Equivalent Grades of Nimonic 90A Across International Standards
Nimonic 90A is codified under multiple national and international specification systems. The table below maps its designations and governing standards across major markets. Fushun Metal certifies to all listed specifications and can dual-certify heats where required.
| Country / System | Designation | Key Standards |
|---|---|---|
| USA (AMS) | Nimonic 90A / Alloy 90 | AMS 5829, AMS 5716, AMS 5549, AMS 5582 |
| USA (ASTM/ASME) | N07090 | ASTM B637, ASME SB637 |
| Germany (DIN/W.Nr.) | 2.4632 / NiCr20Co18Ti | DIN 17742, DIN 17754, EN 10095 |
| United Kingdom (BS) | Nimonic 90 / NA 19 | BS HR 1, BS HR 2, BS HR 501, BS HR 502, BS HR 503, BS 3075 |
| France (AFNOR) | NCK 20TA | NF A54-301 |
| China (GB) | GH4090 / GH90 | GB/T 14992 |
| Japan (JIS) | NW 7090 | JIS G 4901 |
| International (ISO) | NiCr20Co18TiAl | ISO 9724, ISO 9725 |
Applications of Nimonic 90A
Nimonic 90A is specified wherever high creep-rupture life, fatigue strength, and oxidation resistance must be maintained simultaneously in the 650–920°C range. Its high gamma-prime volume fraction and excellent hot-hardness retention make it the alloy of choice for rotating and dynamically loaded hot-end components across aerospace, power generation, and high-performance automotive sectors.
Gas Turbine Hot Section
High-pressure turbine blades, nozzle guide vanes, turbine discs, shroud rings, interstage seals, and hot-gas-path structural rings for aero-derivative and industrial gas turbines.
Turbocharger Components
Turbocharger rotors, turbine wheels, shaft-and-wheel assemblies for high-performance automotive, marine, and heavy-duty diesel engines operating at sustained exhaust gas temperatures above 850°C.
High-Temperature Fasteners & Springs
Turbine casing bolts, hot-section studs, valve springs, Belleville washers, retaining rings, disc lock plates, and spring-temper wire for dynamic applications up to 550°C in aged condition.
Internal Combustion Engines
Exhaust valves, valve seat inserts, pre-combustion chamber components, and glow-plug sheaths for high-output diesel and natural-gas reciprocating engines in marine and stationary power applications.
Nuclear & Power Generation
Steam generator tube supports, reactor internal springs, hold-down bolts, control rod guide bushings, and high-temperature instrumentation fittings for nuclear and conventional power plants.
Hot Work Tooling & Dies
Hot-forging die inserts, extrusion tooling, die-casting cores and inserts, hot-shear blades, and forming mandrels for elevated-temperature metalworking processes.
Nimonic 90A — Supply Range by Fushun Metal
Fushun Metal stocks and processes Nimonic 90A across all major mill forms from a single integrated facility. Our in-house 6000-ton hydraulic open-die press, 1800-ton precision radial forger (GFM), and multi-stand 850/550/350/250 rolling mills enable a broad dimensional envelope without outsourcing—ensuring uninterrupted lot traceability from melt to delivery under ISO 9001 and AS9120B. Material is supplied in the solution-annealed condition per BS HR 1 / AMS 5829, ready for machining, forming, or subsequent precipitation hardening by the customer. All forged products are ultrasonic tested to AMS 2375 Class A and accompanied by mill test certificates to EN 10204 3.1 or 3.2 as required.
Rolled Round Bar
Diameter 8 mm – 250 mm. Length 2,000 – 6,000 mm. Solution-annealed per BS HR 1 / AMS 5829. Centerless ground to h8/h9 tolerance. Supplied as straight random lengths or precision cut-to-order.
Rolled Flat Bar
Thickness 3 mm – 50 mm, width 10 mm – 350 mm. Length up to 4,000 mm. Hot-rolled and annealed surface finish. Edge-conditioned: sheared, sawn, or chamfered per customer drawing.
Forged Round Bar
Diameter 80 mm – 750 mm. Length 1,000 – 7,000 mm. Open-die forged on 1800t/6000t presses with controlled reduction ratios. Rough-turned or finish-machined. UT inspected to AMS 2375 Class A.
Forged Flat / Disc / Ring
OD / width 150 mm – 1,400 mm. Thickness 20 mm – 450 mm. Single-piece weight up to 5,000 kg. Contour-forged rings, rolled rings, and pancake discs available. Rough-machined with UT and dye-penetrant inspection.
Chemical Composition of Nimonic 90A — BS HR 1 / AMS 5829
All heats produced by Fushun Metal are melted via VIM+VAR or VIM+PESR and verified against the composition limits below by optical emission spectrometry and LECO combustion analysis. Full chemical certificates are issued with every shipment under ISO 9001 and AS9120B quality management. The tightly controlled aluminum-to-titanium ratio and the nominal 18% cobalt content are critical—cobalt raises the gamma-prime solvus temperature to approximately 985–1010°C, directly governing the maximum service temperature and long-term microstructural stability of the alloy.
| Element | C | Cr | Ni | Co | Al | Ti | |
|---|---|---|---|---|---|---|---|
| Wt.% | ≤0.13 | 18.0–21.0 | Bal. | 15.0–21.0 | 1.0–2.0 | 2.0–3.0 | |
| Element | Fe | Mn | Si | Cu | S | B | Zr |
| Wt.% | ≤1.5 | ≤1.0 | ≤1.0 | ≤0.20 | ≤0.015 | ≤0.020 | ≤0.15 |
Mechanical Properties of Nimonic 90A — Per Product Form
The values below represent minimum guaranteed properties in the fully heat-treated condition: solution treatment at 1080°C ± 10°C (rapid air or oil quench), followed by precipitation aging at 700°C ± 10°C for 16 hours (air cool), per AMS 5829 / BS HR 1. This standard heat treatment cycle produces the optimal balance of room-temperature tensile strength, elevated-temperature creep-rupture life, and ductility for rotating and dynamically loaded hot-end components.
Fushun Metal performs all heat treatment in-house under calibrated furnace controls and Nadcap-compliant procedures. For spring-temper wire applications requiring maximum fatigue life in service up to 550°C, an alternative aging schedule of 750°C for 4 hours (air cool) can be applied. Material can be supplied in the solution-annealed condition for customer-side forming and subsequent precipitation hardening, or in the fully aged condition ready for finish machining.
Physical constants: Density 8.18 g/cm³; Melting range 1335–1370°C; Hardness 248–311 HB (aged condition); Modulus of elasticity 213 GPa at 20°C; Thermal conductivity 11.7 W/m·K at 20°C; Coefficient of thermal expansion 12.3 μm/m·°C (20–100°C). The alloy is essentially non-magnetic in the annealed and aged conditions.
| Product Form | Test Temp. (°C) | Tensile Strength (MPa) | Yield Strength (MPa) | Elongation (%) | Hardness (HB) |
|---|---|---|---|---|---|
| Bar & Forgings | 20 | ≥950 | ≥600 | ≥20 | 248–311 |
| Bar & Forgings | 700 | ≥620 | ≥520 | ≥15 | — |
| Sheet & Strip | 20 | ≥950 | ≥600 | ≥20 | — |
| Spring Wire (Aged) | 20 | ≥1200 | ≥800 | ≥10 | 400–450 HV |
| Seamless Tube | 20 | ≥950 | ≥600 | ≥20 | — |