Standard Steel Grade
Chemical Composition %
C: Mn: Si: P: S: Cr: Mo: Ni: V: W: Co:
PN SW7M
0.82 – 0.92 <0.4 <0.5 <0.03 <0.03 3.5 – 4.5 4.5 – 5.5 <0.4 1.7 – 2.1 6.0 – 7.0 <0.5
ISO HS6-5-2C
0.86 – 0.94 <0.4 <0.45 <0.03 <0.03 3.8 – 4.5 4.7 – 5.2 – 1.7 – 2.1 5.9 – 6.7 –
ISO HS6-5-2 – 1.3339
0.80 – 0.88 <0.4 <0.45 <0.03 <0.03 3.8 – 4.5 4.7 – 5.2 – 1.7 – 2.1 5.9 – 6.7 –
DIN S6-5-2 – 1.3343
0.86 – 0.94 <0.4 <0.45 <0.03 <0.03 3.8 – 4.5 4.7 – 5.2 – 1.7 – 2.0 6.0 – 6.7 –
NF Z85WDCV06-05-04-02
0.80 – 0.87 <0.4 <0.5 <0.03 <0.03 3.5 – 4.5 4.6 – 5.3 – 1.7 – 2.2 5.7 – 6.7 –
ASTM UNS T11302 – AISI M2
0.78 – 0.88 0.15 – 0.40 0.20 – 0.45 <0.03 <0.03 3.75 – 4.50 4.5 – 5.5 – 1.75 – 2.20 5.50 – 6.75 –
GOST R6M5 – Р6М5
0.82 – 0.90 <0.5 <0.5 <0.03 <0.25 3.80 – 4.40 4.8 – 5.3 <0.4 1.7 – 2.1 5.5 – 6.5 <0.5

 

S6-5-2, HS6-5-2, 1.3343 – specification and application

High-speed steel with very good efficiency, ductility, resistance to abrasion and torsion, and impact strength used to work with products with a strength of more than 830 MPa. It is used in the production of drills, blades, knives, spiral drills, thread cutting tools, broaching tools, gear tools, milling cutters, mandrel reamers, end milling cutters, and circular saw segments. SW7M / 1.3343 is prone to decarburization and overheating during heat treatment. After hardening and tempering, it achieves hardness above 63 HRC.

Mechanical properties of SW7M, S6-5-2, HS6-5-2C, 1.3343

  • Hardness in +A delivery condition: <269 HB

 

  • Hardness in +A+C delivery condition: <319 HB

 

  • Hardness in +A+CR delivery condition: <339 HB

 

  • Hardness after hardening and tempering:
    • at 300 ℃ = 61,5 HRC

 

  • at 350 ℃ = 62 HRC

 

  • at 400 ℃ = 62 HRC

 

  • at 450 ℃ = 63 HRC

 

  • at 500 ℃ = 65 HRC

 

  • at 550 ℃ = 65 HRC

 

  • at 600 ℃ = 60 HRC

 

  • at 650 ℃ = 52 HRC

 

Heat and plastic treatment processes of SW7M, S6-5-2, HS6-5-2C, 1.3343 steel:

  • Softening annealing at a temperature of 800 – 900 ℃

 

  • Relief annealing at a temperature of 600 – 700℃

 

  • Heating no. I in a temp. of about 550℃

 

  • Heating no. II in a temp. of about 850℃

 

  • Austenitizing at 1190 – 1230 ℃ (hardening in salt bath and oil)

 

  • Tempering usually in the range of 550 – 570 ℃

 

  • Forging and rolling at temperatures 1100 – 900 ℃

 

  • Nitriding in the temperature range of 510 – 530 ℃

 

In the above mentioned grades the company provides:

  • Drawn bars, hot-rolled bars, high-speed forged bars 1.3343, HS6-5-2, S6-5-2, HS6-5-2C

 

  • High-speed steel sheets 1.3343, HS6-5-2, S6-5-2, HS6-5-2C

 

Other replacements and equivalents of the grade:

SW7M, 1.3343, HS6-5-2C, HS6-5-2, S6-5-2, 1.3339, X82WMOCRV6-5-4, X80WMOCRV6-5-4, X 82 WMOCRV 6-5-4, X 80 WMOCRV 6-5-4, R6M5, AISI M2, SKH51, SS 2722, R6, W6MO5CR4V2, CSN 19830, 1.3553, SC6-5-2, SC 6-5-2, 1.3341, BS BM2, X82WMO0605KU, X 80 WMO 06 05 KU, RP5, EM2, F-550.A, UNS T11302, AISI M-2, HS 6-5-2 C, S 6-5-2, Р6М5, R6M5.

 

About Us

Founded in 1998, FuShun covers an area of 3000 square meters, annual sales volume of 20000 tons. We are engaged in the manufacture and export of Tool Steel, Nickel Alloy, Stainless Steel and other special steel products…,View more content About Me.

Contact Lists

General Manager: Ms. Florence

[email protected]

Get A Free Quote!

Find your steel grade and get a quote today.

NOW Send Your Inquiry To : [email protected]

x