manufacturer of nickel alloy, stainless steel, tool steel, alloy steel

1.2329, 46CrSiMoV7, Hot Work Tool Steel

1.2329, 46CrSiMoV7, Hot Work Tool Steel

General

1.2329 is a chromium-nickel-molybdenum-vanadium alloyed hot work tool steel which is characterized by:

  • Good toughness
  • Good resistance to high thermal stresses
  • Good stability in hardening
  • Good through-hardening properties
Typical

analysis %

C

0.45

Si

0.7

Mn

0.8

Cr

1.8

Ni

0.5

Mo

0.3

V

0.2

Standard

specification

W.-Nr. 1.2329,  DIN 46 CrSiMoV7
Delivery

condition

Soft annealed to max. 250 HB.
Colour code Red/black

Cutting:

Precision cutting to standard dimensions

Custom cutting according to client specifications

 

Surface Grinding/Polishing:

Thickness tolerance: -0 to +0.1mm

Flatness: 0.01/100mm

Surface roughness: Ra ≤1.6 or Rz ≤6.3

 

Applications

1.2329 is ideally suited for support parts for extrusion tooling, e.g. wedge blocks and bolsters.

 

Properties

Hardened and tempered to hardness 40 HRC. Data at room and elevated temperatures.

Temperature 20°C

(68°F)

200°C  (390°F) 400°C

(750°F)

Density

kg/m3

lbs/in3

 

7 780

0.281

 

7 730

0.279

 

7 670

0.277

Coefficient of

thermal expansion

per °C from 20°C

per °F from 68°F

 

 

 

12.9 x 10–6

7.1 x 10–6

 

13.6 x 10–6

7.5 x 10–6

Modulus of elasticity

N/mm2

psi

 

205 000

29.7 x 106

 

195 000

28.3 x 106

 

180 000

26.1 x 106

Thermal conductivity*

W/m°C

Btu in(ft2h°F)

 

30

211

 

31

218

 

30

211

 

Heat treatment

Soft annealing

Protect the steel and heat through to 780°C (1435°F). Then cool in the furnace at 15°C

(25°F) per hour to 650°C (1200°F),then freely in air.

Stress relieving

After rough machining the tool should be

heated through to 650°C (1200°F), holding time 2 hours. Cool slowly to 500°C (930°F), then freely in air.

Hardening

Pre-heating temperature: 600–700°C (1110– 1290°F).

Austenitizing temperature: 880–920°C (1615– 1690°F) normally 900°C (1650°F).

Soaking time 30 minutes. Soaking time = time at hardening temperature after the tool is fully heated through.

Protect the part against decarburization and oxidation during hardening.

Quenching media

  • Air blast/vacuum
  • Martempering bath. Temperature 200–250°C (390–480°F) for max. 15 minutes, then

cooling in air

  • Warm oil

Note:Temper the tool as soon as its tempera- ture reaches 50–70°C (120–160°F).

 

About Us

Founded in 1998, FuShun covers an area of 3000 square meters, annual sales volume of 20000 tons. We are engaged in the manufacture and export of Tool Steel, Nickel Alloy, Stainless Steel and other special steel products…,View more content About Me.