manufacturer of nickel alloy, stainless steel, tool steel, alloy steel

AISI A8 MOD Cold Work Tool Steel

AISI A8 MOD Cold Work Tool Steel

1: AISI A8 MOD steel introduction

A8-mod is a modified version of AISI A8. It’s a conventional cold work tool steel, with a medium carbon content and alloyed with chromium, molybdenum and vanadium. This steel is an improved steel of A8 steel, with good hardenability, toughness, heat treatment dimensional stability. Suitable for punches and cold forging dies with hardness requirements of 55-60 HRC. In addition, it is suitable for manufacturing non-metallic materials due to good hardness, wear resistance and toughness.

Cutting:

Precision cutting to standard dimensions

Custom cutting according to client specifications

Cold Work Tool Steel Dimensions

We offer premium cold work tool steel in various forms, manufactured with advanced 5000-ton forging press technology for superior density and performance.

Product Form Specifications
Forged Round Bar Dia. up to 1200mm
Forged Flat Bar Thickness 100-600mm, Width 300-2000mm
Rolled Round Bar Dia. 10-200mm
Hot Rolled Plate Thickness 1-100mm, Width 60-1600mm

 

2: AISI A8 MOD Steel equivalent

Country China Japan Germany USA UK
Standard GB/T 1299 JIS G4404 DIN EN ISO4957 ASTM A681 BS 4659
Grade / / / A8 MOD /

 

3: AISI A8 MOD steel chemical composition

Grade C Mn P S Si Cr V Mo
A8 MOD 0.50 0.30 0.03 0.03 0.95 8.01 0.50 1.45

 

4: AISI A8 MOD steel mechanical properties

The mechanical properties mainly include tensile strength, yield strength, elongation, area or reduction, hardness, impact value, non-metalic inclusion etc. Different heat treatment, the mechanical properties will be different, such as normalized, tempered, QT.

 

6. AISI A8 MOD Tool Steel Heat Treatment

Annealing

Slowly heat to 870 – 890 ℃ , then slowly Cool to 500 ℃ in heat treatment furnace. Then frosty in make public. After annealing hardness HBS: 229 Max

Quenching 

Quenching temperature / ℃ | outlet air cooling, oil cooling or air cooling : 1000 – 1050

Quenching hardness : 59-62 HRC

Tempering 
Tempering temperature / ℃ : 150 – 320

After tempering hardness HRC or future: 53 – 60

 

7: Delivery condition
For hot forged or hot rolled bar, usually the delivery condition is hot forged or rolled, annealed, rough turned.
For hot forged plate, usually the delivery condition is hot forged, annealed, milled surface.

For hot rolled plate, usually the delivery condition is hot rolled, annealed, black surface.

 

About Us

Founded in 1998, FuShun covers an area of 3000 square meters, annual sales volume of 20000 tons. We are engaged in the manufacture and export of Tool Steel, Nickel Alloy, Stainless Steel and other special steel products…,View more content About Me.