manufacturer of nickel alloy, stainless steel, tool steel, alloy steel

Incoloy 926 / 1.4529 / N08926: A 1780 Hot Strip Mill Just Proved China’s Super-Austenitic Window Is Open

Incoloy 926 / 1.4529 / N08926: A 1780 Hot Strip Mill Just Proved China’s Super-Austenitic Window Is Open

When Anyang Steel’s No. 2 continuous-rolling shop reported its first successful run of S38926 on a 1780 mm hot-strip line, most trade coverage framed it as “one more high-end grade added to the catalogue.” That reading misses the point. The grade does not need another cheerleader; the super austenitic stainless steel family has been spec’d into seawater and sour-service for decades. What is genuinely new is that a production line designed around carbon and low-alloy grades held a narrow hot-working window tight enough to roll a 6 %-molybdenum alloy and keep both shape and surface inside tolerance. That is a process-capability signal, and for buyers of corrosion-resistant plate it changes the supply arithmetic.

1. The Grade and Its International Equivalents

S38926 is the Chinese designation for a high-alloy austenitic stainless steel that the rest of the world sells under alloy names tied to its chemistry: roughly 25 % nickel, 20 % chromium, 6.5 % molybdenum, with nitrogen and copper completing the package. Outside China it is listed as UNS N08926, EN 1.4529 (X1NiCrMoCuN25-20-7), and most commonly by the trademark Incoloy 926 or the shorthand 25-6Mo. Japan carries it as SUS N08926; Russia lists 01Kh25N22AMB-class equivalents. There is no separate “Chinese secret” here — the grade is the same material with a domestic stamp, which is exactly why a buyer can cross-check chemistry and properties against ASTM B625 / B677 and EN 10028-7 without translation risk.

System Designation Note
China (GB/T) S38926 Source grade in the news
USA (UNS / ASTM) N08926 / B625, B677 ASTM A240 also applies for plate
Europe (EN / WNR) 1.4529 / X1NiCrMoCuN25-20-7 EN 10028-7, VdTÜV 502
Trademark Incoloy 926, 25-6Mo, UR 926 Outokumpu / Industeel / SMC
Japan (JIS) SUS N08926 Approximate, not a separate grade
Family neighbour 254 SMO (S31254 / 1.4547) Same 6Mo class, slightly lower Ni
Element S38926 (wt%) ASTM B625 limit Role
C ≤0.020 ≤0.020 Blocks intergranular corrosion
Cr 19.0-21.0 19.0-21.0 Passive film, oxidation
Ni 24.0-26.0 24.0-26.0 Austenite stability, SCC resistance
Mo 6.0-7.0 6.0-7.0 Pitting / crevice core
Cu 0.5-1.5 0.5-1.5 Reducing-acid (H2SO4) tolerance
N 0.15-0.25 0.15-0.25 Strength + austenite stabilizer

2. Why “Super” Is a Corrosion Number, Not a Marketing Word

The PREN of a stainless steel is a back-of-envelope sum — %Cr + 3.3×%Mo + 16×%N (or 30×%N in the stricter ASTM G48 reading). 316L lands near 25, 904L near 35, and 254 SMO near 43. S38926 sits at roughly 43-47, which is the threshold engineers use to call a grade “super austenitic.” In plain terms: in a chlorides-and-acid environment where 316L fails in hours, this grade is designed to run for years. The CPT — the temperature at which pitting starts in ferric-chloride test — is quoted at 65°C and above, against 316L’s ~10°C. That gap is the entire reason the grade exists.

Grade Mo class PREN CPT (°C) Typical use
316L 2Mo ~25 ~10 General service
904L 4Mo ~35 ~43 Sulfuric acid, upgrade from 316
254 SMO 6Mo ~43 ~65 Seawater, FGD
S38926 / 926 6Mo + Cu 43-47 ≥65-85 Sour oil & gas, desalination
Inconel 625 Ni-base ~48 ~90 Nickel alloy benchmark
Property (annealed) S38926 / 926 316L Edge
Tensile Rm (MPa) ≥650 ≥520 +25 %
Yield Rp0.2 (MPa) ≥295 ≥210 +40 %
Elongation (%) ≥35 ≥40 Comparable
Hardness (HB) ≤220 ≤217 Similar
Density (g/cm³) 8.1 8.0 Similar

3. The Real Story Is in the Rolling, Not the Recipe

Here is the part most readers skip. The chemistry of S38926 has been stable for thirty years; what makes it hard to produce is hot ductility window — the narrow band of temperature where the slab can be deformed without cracking — and its high deformation resistance at rolling temperature. With 25 % nickel and 6.5 % molybdenum, the alloy’s flow stress is far above that of carbon steel, and its safe hot-working range (roughly 1200 down to 900 °C, then quench) is tight compared with ordinary stainless. Sit in the 600-900 °C band too long and brittle intermetallic phases precipitate; overheat past incipient melt and the slab is scrap. Holding that window on a continuous hot-strip line — where the equipment was sized for carbon steel — is the actual engineering achievement.

Difficulty Root cause What Anyang’s run had to control
Narrow hot window High Ni + Mo shifts γ stability Heating schedule tuned to 1100-1150 °C soak
High deformation resistance ~2× flow stress of 316L Mill load check, pass reduction matched to stand
Phase precipitation σ / chi in 600-900 °C Cooling path keeps strip out of the band
Shape & surface High roll-force, scale control Roll-gap, pacing and descaling tuned per trial
Consistency Window closes fast off-target Same parameters carried to repeat heats

4. What a 1780 Hot-Strip Mill Rolling It Actually Means

The 1780 line is not a specialty forge; it is a high-volume strip mill. When such a line clears S38926 on a first attempt with plate shape and surface inside spec, the message to the market is not “China made another grade” — it is “the volume base can now absorb high-alloy chemistry without a dedicated mill.” For an overseas buyer that reframes the cost conversation. Specialty mills price super-austenitic plate as a low-volume, high-margin item. A continuous line that has proven the window can push the same chemistry toward batch production, which is where the 904L-to-926 and 316L-to-926 upgrade cases stop being budget exceptions and start being procurement defaults. The next line in the announcement — “move toward stable batch supply” — is the part that matters commercially.

5. Where the Grade Actually Earns Its Keep

S38926 / Incoloy 926 is specified where chloride, acid and pressure meet at the same time. It is the default candidate for seawater reverse-osmosis and multi-stage flash desalination, flue-gas desulfurization absorbers and spray headers, sour oil-and-gas handling, and phosphoric / sulfuric acid plants. The copper addition is what lets it shrug off reducing acids that plain 6Mo grades handle worse.

Sector Component Why 926 over 316L / 904L
Desalination HP membrane shell, piping PREN >43 in brine
FGD Absorber, spray header Acid + chloride slurry
Sour oil & gas Downhole, flowline H2S + Cl- per NACE
Chemical H2SO4 / H3PO4 vessels Cu aids reducing acid
Offshore Seawater fire, ballast Long-life, low maintenance

6. Four Checks Before You Specify 926

  1. Ask for the mill’s actual hot-rolling window, not just the certificate chemistry. A first successful run is real; batch consistency is what protects your job.
  2. Confirm the MTC reports PREN and, where relevant, a CPT test per ASTM G48 — chemistry alone does not prove the corrosion number.
  3. Treat 926 as a 904L upgrade, not a 316L upgrade. The cost step from 316L is large; from 904L it is modest and the gain is real.
  4. Watch the welding procedure. ERNiCrMo-3 (Inconel 625 class) filler, low heat input, interpass below 100 °C — the same tight window logic applies in fabrication.
Harris · Metallurgical Technician, FUSHUN METAL
Source: Anyang Steel No. 2 Continuous-Rolling Shop press release, Aug 2026; grade data cross-checked against ASTM B625 / EN 10028-7 and producer datasheets (Outokumpu, Industeel, Sandmeyer).

About Us

Founded in 1998, FuShun covers an area of 3000 square meters, annual sales volume of 20000 tons. We are engaged in the manufacture and export of Tool Steel, Nickel Alloy, Stainless Steel and other special steel products…,View more content About Me.