manufacturer of nickel alloy, stainless steel, tool steel, alloy steel

Spring Steel Flat Bar

FUSHUN SPECIAL STEEL · Spring Steel · Flat Bar

Spring Steel Flat Bar: Grades, Sizes & Properties

Spring steel flat bar is rolled to a rectangular section and supplied either annealed for forming or quenched and tempered to a hardness band. The section is chosen so that the spring can be formed from bar rather than machined from plate — the rolling tolerance and the edge condition decide whether that works.

3–60 mm
Thickness
20–300 mm
Width
980–1,130 MPa
Tensile, hardened
65Mn / 60Si2Mn / 50CrV
Main grades

Spring steel flat bar: How the Families Differ

Leaf springs, parabolic springs and heavy coil springs are made from flat bar, and the bar is rolled to a section close to the finished spring. That saves machining but puts the tolerance under pressure: a 0.2 mm variation in thickness across the width changes the rate of a leaf spring measurably, and a rolled edge with a seam becomes the fatigue origin.

The grades divide by hardenability and by temper resistance. 65Mn is the volume grade for automotive leaf springs; 60Si2Mn adds silicon for a higher elastic limit and better sag resistance; 50CrV adds chromium and vanadium for springs that run warm or see a high stress amplitude.

Spring steel flat bar is spring steel: the part is designed to deflect and return, so the properties that matter are the elastic limit, the fatigue resistance and the surface condition — not hardness alone. The steel is supplied annealed for forming, or hardened and tempered to a stated band.

Silicon raises the elastic limit and the sag resistance; chromium and vanadium hold hardness at temperature and refine the grain. That is why the alloyed grades carry 30 % more tensile than the plain carbon grades at the same section.

The Two Mistakes That Keep Coming Back

Ordering by grade without the thickness tolerance: two bars of the same grade and different tolerance make springs with different rates, and the difference shows up on the test rig.

Shot-peening a bar with a rolled-in seam: the peening hides the seam for a while, then the spring fails from underneath it.

What buyers get wrong
  • Buying tempered strip and forming a tight radius; the strip cracks at the bend.
  • Specifying hardness without the tempering temperature; the same HRC from different tempers behaves differently in fatigue.
  • Ignoring the edge condition; a sheared edge carries micro-cracks straight into the fatigue section.
  • Assuming annealed strip has no decarburisation; it has to be measured, not assumed.

Selection Matrix

Table 1 — Grade selection by duty

Duty 65Mn 60Si2Mn 50CrV4
Automotive leaf spring Recommended Usable Usable
High sag resistance Usable Recommended Usable
Service to 250 °C Avoid Usable Recommended
Fatigue-critical Usable Usable Recommended

The matrix assumes a hardened and tempered bar; an annealed bar is for forming only and has none of these properties.

Grades We Supply

The grades below are the ones we roll and cut most often. Each one is a different compromise on the same three axes — hardenability, toughness and cost — and the last column says which duty each was designed for.

Table 2 — Grades supplied, with the duty each one covers

Grade C Mn Si Cr V Duty
65# 0.62–0.70 0.50–0.80 0.17–0.37 ≤0.25 — General leaf springs
70# 0.62–0.75 0.50–0.80 0.17–0.37 ≤0.25 — Higher load leaf springs
85# 0.82–0.90 0.50–0.80 0.17–0.37 ≤0.25 — Wear-resistant spring strips
65Mn 0.62–0.70 0.90–1.20 0.17–0.37 ≤0.25 — Automotive leaf springs
60Si2Mn 0.56–0.64 0.60–0.90 1.50–2.00 ≤0.35 — High elastic limit, sag resistance
50CrV4 0.47–0.55 0.70–1.10 0.15–0.35 0.90–1.20 0.10–0.20 Warm service, fatigue
Spring steel flat bar — Tempering response of the three grades
Figure 1 — Spring steel flat bar — Oil quenched from the recommended temperature, tempered 2 h

Supply Range and Tolerances

Supply is quoted by section and length, in coils, bundles or cut lengths, with the straightness and the edge condition stated.

Table 3 — Supply range and tolerances

Form Range Condition
Flat bar 3–60 mm thick × 20–300 mm wide Annealed or Q&T
Square bar 6–100 mm Annealed or Q&T
Coil / bundle Up to 3 t per bundle Strapping to the drawing
Length 3–12 m, or cut to length —

Bar is supplied in bundles up to 3 t, strapped and tagged. Cut lengths are deburred and packed in wooden cases; the straightness class is agreed at order.

Properties That Decide the Choice

Properties are quoted in the hardened and tempered condition, with the tempering temperature stated. The same grade in the annealed condition is meant for forming only.

Table 4 — Properties that decide the selection

Grade Rm (MPa) Rp0.2 (MPa) A5 (%) Hardness
65# ≥980 ≥785 ≥9 269–321 HB
70# ≥1,030 ≥835 ≥8 285–341 HB
85# ≥1,130 ≥980 ≥6 302–363 HB
65Mn ≥980 ≥785 ≥8 269–321 HB
60Si2Mn ≥1,200 ≥1,050 ≥6 321–375 HB
50CrV4 ≥1,250 ≥1,100 ≥7 330–390 HB

Chemical Composition

Carbon sets the hardness after quench, silicon raises the elastic limit, and chromium and vanadium hold the temper at working temperature.

Table 5 — Chemical composition, wt. %

Grade C Si Mn Cr Mo Ni V
65Mn 0.62–0.70 0.17–0.37 0.90–1.20 ≤0.25 — ≤0.25 —
60Si2Mn 0.56–0.64 1.50–2.00 0.60–0.90 ≤0.35 — ≤0.25 —
50CrV4 0.47–0.55 0.15–0.35 0.70–1.10 0.90–1.20 0.10–0.20 ≤0.25 —

Heat Treatment

Austenitise, quench, temper to the specified band. The tempering temperature, not the hardness alone, is what has to be recorded.

Table 6 — Heat treatment schedule

Step Temperature Time / atmosphere Cooling
65Mn 830 °C Oil quench, temper 540 °C Oil
60Si2Mn 860 °C Oil quench, temper 480 °C Oil
50CrV4 850 °C Oil quench, temper 520 °C Oil
Spring steel flat bar — Section capability
Figure 2 — Spring steel flat bar — What can be rolled and what has to be machined

How These Grades Fail

Flat bar springs fail at the edge. The rolled edge carries seams and decarburisation, and both are crack starters under the bending stress. That is why the edge condition is specified separately from the grade.

The second failure is sag. A spring that runs at 250 °C loses load as the temper backs off; 50CrV4 resists it, 65Mn does not.

Certificate and Testing

  • EN 10204 3.1 mill certificate with chemistry and mechanical properties, heat number and melt route.
  • Hardness survey and dimensional report on every piece on request.
  • Ultrasonic inspection to ASTM A388 or SEP 1921 where the section or the application calls for it.
  • Third-party inspection — SGS, BV, TUV — arranged before dispatch, at the customer’s instruction.
  • Spectro check on the finished part where a weld or a heat treatment has been added after despatch.

Packing, MOQ and Delivery Terms

Bundles are strapped with steel band and marked with grade, heat number, section and net weight. Export packing is seaworthy, with the bar ends protected.

Table 7 — Trade terms, packing and documents

Item Standard terms
Trade terms FOB Shanghai / CIF / CFR / EXW; FOB is the default.
Minimum order One bundle, plate or coil for stock sizes; mill runs quoted individually.
Lead time 20–30 days from order confirmation for stock sizes; 30–45 days where forging or heat treatment is included.
Payment 30 % T/T deposit, 70 % against the bill of lading copy; L/C at sight above 20 t.
Packing Seaworthy export packing — crated or strapped, marked with grade, heat number, size and net weight.
Documents EN 10204 3.1 certificate, packing list, invoice, bill of lading, certificate of origin; legalisation on request.

Frequently Asked Questions

Which grade for an automotive leaf spring?

65Mn is the volume choice; 60Si2Mn where the spring needs a higher elastic limit and better sag resistance.

Can you supply hardened and tempered bar?

Yes, to the hardness band on this page, with the tempering temperature recorded on the certificate.

What is the thickness tolerance?

To the EN 10092 table or to the drawing; the tolerance is agreed at order because it affects the spring rate.

Is 50CrV4 available?

Yes, in the size range shown, annealed or quenched and tempered.

Do you supply cut lengths?

Yes, 3–12 m as standard, cut to length on request.

Spring steel flat bar bundle
Figure 3 — Spring steel flat bar, bundled and tagged by heat number

Related Grades

Browse the full range: spring steel grades.

Request a Quote

Five lines are enough to quote
  • Grade and governing standard
  • Form, size and quantity
  • Delivery condition and hardness
  • Certificate and testing requirements
  • Destination port and required date

Email [email protected] or use the form below. Drawings in DXF, STEP or PDF are all fine. Stock sizes ship within 20 days of order confirmation.

About Us

Founded in 1998, FuShun covers an area of 3000 square meters, annual sales volume of 20000 tons. We are engaged in the manufacture and export of Tool Steel, Nickel Alloy, Stainless Steel and other special steel products…,View more content About Me.

Contact Lists

General Manager: Ms. Florence

[email protected]

Get A Free Quote!

Find your steel grade and get a quote today.

NOW Send Your Inquiry To : [email protected]