manufacturer of nickel alloy, stainless steel, tool steel, alloy steel

AISI 4140 Alloy Steel

Alloy structural steel · Cr-Mo · 4140

AISI 4140 Alloy Steel (42CrMo4 / 1.7225)

The chromium-molybdenum steel most shafts, gears and bolts are made from. 0.40 % carbon, 1 % chromium, 0.2 % molybdenum. It hardens through 100 mm in oil, holds 300 HB at 30 HRC, and gets its temper resistance from the molybdenum rather than the carbon.

0.38–0.43 C
Base chemistry
Ø1200 mm
Max forged bar
28–32 HRC
Typical Q+T
EN 10204 3.1
Every lot
Download datasheet (PDF)One page: designation, chemistry, mechanical properties, supply range and inspection scope.

At a glance

Item Detail
Designations AISI 4140 / UNS G41400 / 42CrMo4 / 1.7225 / SCM440
Standards ASTM A29, A322, A193 B7; EN 10083-3
Delivery condition Annealed max 250 HB, or quenched and tempered to your window
Melt route EAF + ladle refining + vacuum degassing; ESR on request
Typical use Shafts, gears, connecting rods, A193 B7 bolts, mould bases, hydraulic rods
Certificate EN 10204 3.1 with chemistry, hardenability and mechanical results

Why 4140 and not 1045 or 4340

The molybdenum is what separates 4140 from a plain 0.4 % carbon steel. It suppresses temper embrittlement, so a shaft quenched and tempered to 30 HRC stays there through service at 300 °C, where 1045 would soften and start to embrittle at the grain boundaries. It also buys depth of hardening: oil quenching gives full hardness to roughly 60–100 mm diameter, which covers most shaft work without going to a more expensive alloy.

Against 4340 the difference is nickel, and it is expensive. 4340 carries 1.65–2.00 % Ni and hardens through 150 mm, with better toughness at the same strength — but it distorts more in quench and costs roughly twice as much. Under 100 mm section, in bending or torsion rather than pure tension, 4140 is the right answer and we will say so before you order.

For pressure bolting the same steel is bought as A193 B7, which fixes the chemistry and the minimum tempering temperature at 620 °C. B7 and B7M come off the same heats, and the grade marking on the bar and the 3.1 certificate both carry the B7 designation rather than the mill grade.

Supply range and delivery condition

Form Size range Condition
Rolled round bar Ø10–200 mm As rolled / annealed / Q+T
Forged round bar Ø80–1200 mm Annealed / Q+T
Forged flat bar Thickness 100–600 mm × width 300–2000 mm Annealed
Rolled wire rod Ø5.5–20 mm As rolled / annealed

Sawn and squared within these ranges. Hollow bar and rough-machined tube shells quoted on request.

Chemical composition

C Si Mn P S Cr Mo
0.38–0.43 ≤0.35 0.75–1.00 ≤0.035 ≤0.040 0.80–1.10 0.15–0.25

AISI 4140 to ASTM A29. The EN 42CrMo4 window differs slightly — Cr 0.90–1.20, P 0.025 and S 0.035 max. Tell us which one the drawing calls for.

Mechanical properties you can design to

Condition Tensile MPa 0.2 % proof MPa Elongation % Hardness
Annealed 655 415 25.7 197 HB
Q+T, 28–32 HRC 950–1100 750–900 14–18 300 HB
Q+T, 35 HRC 1150–1250 950–1050 10–13 340 HB
A193 B7 minimum 860 725 16 ≤35 HRC

Section size matters. The figures above apply to bar up to 100 mm; larger sections are tested at the quarter point and reported as such on the certificate.

Heat treatment

Normalising 870–900 °C, air cool. Annealing 840–870 °C, furnace cool to 250 HB max. Hardening 830–860 °C, oil quench; water only under 25 mm and with the cracking risk understood.

Tempering one hour per 25 mm of section, one hour minimum, air cool. 300 HB needs about 540 °C, 340 HB about 480 °C. Temper twice on anything with a stress concentration, and stay out of the 250–400 °C band — that is the embrittlement trough for this family even with the molybdenum present.

What ships with every lot

  • EN 10204 3.1 mill certificate — chemistry, mechanical properties and the heat number
  • Ultrasonic inspection to SEP 1921 / ASTM A388 on request
  • Hardness survey across the section on request
  • Grain size to ASTM E112 on request
  • ESR or remelt route where the application needs it

Cutting, machining and surface

Operation What we hold
Saw cutting Section up to 1200 mm; square within 1 mm per 100 mm
Surface grinding Thickness tolerance −0 to +0.1 mm; flatness 0.01/100 mm
Milling Bright milled, six faces squared
Vacuum heat treatment Hardening and double tempering to your window
CNC / deep drilling Quoted from drawing — DXF, STEP or PDF

Packing and delivery

Bars are bundled by heat number, end-painted with grade and heat number, and strapped to wooden skids. Blocks travel in plywood cases with the machined faces protected. Every package is stencilled to match the certificate inside.

Typical lead time 20–30 days on stock sizes, 30–40 days for quenched and tempered bar where the mechanical test has to be run and reported. Loading from Shanghai, Qingdao or Shenzhen, FOB or CIF.

4140 bar in stock — heat number and diameter (Ø145) stencilled on the sawn ends, matching the 3.1 certificate.
4140 bar in stock — heat number and diameter (Ø145) stencilled on the sawn ends, matching the 3.1 certificate.

Request a quote

Send these five lines and we quote within one working day
  • Grade and standard — 4140 to ASTM A29, 42CrMo4 to EN 10083-3, or A193 B7
  • Form and size — diameter and cut length, or thickness × width × length
  • Quantity in pieces or kilograms
  • Delivery condition — annealed or Q+T, with the hardness or tensile window
  • Inspection — 3.1, UT, Jominy curve or grain size

Email [email protected]  or use the form below. Drawings in DXF, STEP or PDF are all fine.

Related grades

Other mould steel grades from the same mill

One heat-treatment route, one certification route — grades can be combined in a single shipment.

Browse all alloy structural steel grades →

About Us

Founded in 1998, FuShun covers an area of 3000 square meters, annual sales volume of 20000 tons. We are engaged in the manufacture and export of Tool Steel, Nickel Alloy, Stainless Steel and other special steel products…,View more content About Me.

Contact Lists

General Manager: Ms. Florence

[email protected]

Get A Free Quote!

Find your steel grade and get a quote today.

NOW Send Your Inquiry To : [email protected]

x