ALLOY STEEL 9310 AMS 6265 VAR – UNS 93106

9310 is low alloy steel containing nickel, chromium and molybdenum. It has high core hardness and high fatigue strength. This alloy is best machined in the normalized and tempered state. All of this makes 9310 excellent for aircraft parts. 9310 steel specializes in high core strength applications. It also exhibits good strength, high toughness, hardenability, core strength, and very high fatigue strength. When annealed, 9310 has good ductility, machinability, and cold working properties. Additionally, 9310 is easily welded. It is typically used in gears, crankshafts, heavy-duty gears, the automotive, trucking, and aerospace industries.

 

9310 nickel-chrome-molybdenum low alloy steel is melted as AOD + VAR or VIM + VAR melt type.  The alloy additions of nickel, chromium, and molybdenum help give this grade very good strength and toughness .  This grade also has the ability to be case hardened making it an excellent candidate for heavy duty gears and shafts often used in the aircraft industry

 

GENERAL CHARACTERISTICS OF ALLOY STEEL 9310

This is a nickel-chrome-molybdenum case-hardening steel, with good strength and toughness properties. It shows high hardenability, high core hardness and high fatigue strength.

 

SPECS USAP PRODUCES TO:

AMS 6260
AMS 6265
AMS 6267
ASTM A29 (E9310)
ASTM A331 (E9310)
ASTM A519 (E9310)
ASTM A646 (9310-2)
SAE J1397 (9310)
SAE J404 (9310)

 

BENEFITS OF 9310 steel

Normalized & Tempered

Solid strength and toughness properties

High Hardenability, High Core Hardness, and High Fatigue Strength

9310 steel is a low alloy steel that contains Nickel, Chromium, and Molybdenum. Alloy 9310 Bar is a triple alloy based on the inclusion of the previous elements of Nickel, Chromium, and Molybdenum.

 

9310 Vac Melt is a high quality carburizing steel produced by a vacuum consumable electrode process. 9310 has a high hardenability, high core hardness and high fatigue strength. All of those aspects considered, 9310 steel is ideally suited for aircraft engine gear and pinon applications.

 

9310 Alloy Steel is manufactured for the purpose of case hardening and 9310 steel is deep hardening. Generally 9310 steel is most commonly used in applications where toughness, high wear resistance and strength are required.

 

9310 VAR AMS 6265 is a Chromium-Nickel-Molybdenum Alloy used as a Carburizing Grade for Aircraft Parts. Users can obtain high case hardness coupled with high core strength and toughness. High alloy content makes it suitable for use in relatively large cross-sections. Its combination of high alloy and low carbon content can achieve high core hardness with a narrow range between thicker and thinner part cross sections.

 

This alloy can be used in some applications without case-hardening, as it exhibits strength with excellent toughness and ductility. Carburizing offers a highly wear-resistant surface. Service Steel Aerospace stocks Premium Aircraft Quality produced double melted in an Electric Furnace, followed by a VAR, or Vacuum Arc Remelt (also known as CEVM). Standard air-melted Aircraft Quality AMS 6260 Air Melt material is available on request. 9310 VIM-VAR material is also available on request.

 

APPLICATIONS OF 9310 STEEL

Components with large cross section requiring high toughness and core strength such as gears, crankshafts and heavy-duty gear shafts in aircraft and truck construction.

9310 VAR steel is typically used in the following applications:

Aircraft engine gears & pinions

Shafts

Clutch Parts

Boring bars

Piston pins

Aluminum rolling mill rolls

 

Symbol Element Min % Max %
C Carbon 0.07% 0.13%
Mn Manganese 0.40% 0.70%
Si Silicon 0.15% 0.35%
P Phosphorus 0.015%
S Sulfur 0.015%
Cr Chromium 1.00% 1.40%
Ni Nickel 3.00% 3.50%
Mo Molybdenum 0.08% 0.15%
B Boron 0.001% (10 ppm)
Cu Copper 0.035%

 

AISI 9310 STEEL FORGING

This alloy would be forged between 2250 and 1700ºF (1230 and 925ºC.)

 

AISI 9310 STEEL HEAT TREATMENT

Annealing: Not normally annealed: if so sub-critical anneal to give spheroidized structure.

Normalizing: 1650-1700ºF (900-930ºC.)

Carburizing: 1650-1740ºF (900-950ºC) and oil quench.

Hardening: Core: 1530-1620ºF (830-880ºC) and oil quench. Case: 1440-1470ºF (780-800ºC ) and oil quench

Tempering: 340-410ºF (170-210ºC.)

Type Process
Annealing Heat throughout to 1475° – 1575° F, then furnace cool
Normalizing Heat throughout to 1650° – 1750° F, then air cool
Carburizing & Hardening Carburize at 1650° – 1700° F, slow cool. To harden, oil quench from 1425-1545 F
Temper At 250° – 350° F
Approx Case Hardness 60 – 62 HRC
Approx Core Hardness 331 – 363 BHN

 

AISI 9310 STEEL Typical Core Properties after Pseudo-Carburizing:

Heat Treatment Tensile Strength Yield Strength Elongation in 2″ Reduction of Area Core Hardness
Pseudo Carburized 1700° F for 8 hours. Oil quenched, Tempered at 300° F for 2 hours 187 ksi 155 ksi 15% 51% 375 Bhn
Pseudo Carburized 1700° F for 8 hours. Slow cool to room temperature. Heat to 1425° F, oil quench. Tempered at 300° F for 2 hours 155 ksi 130 ksi 15.5% 52% 331 Bhn
Pseudo Carburized 1700° F for 8 hours. Slow cool to room temperature. Heat to 1525° F, oil quench. Tempered at 300° F for 2 hours 175 ksi 155 ksi 16% 53% 363 Bhn

 

Mechanical Information
Density Ultimate Tensile Strength Yield Tensile Strength
Imperial 0.284 lb/in3 132,000 psi 82,800 psi
Metric 7.86 g/cc 907 MPa 571 MPa

 

AISI 9310 STEEL Cold Working

Conventional methods are used to cold work AISI 9310 alloy steel that has good ductility in the tempered and hardened conditions.

 

AISI 9310 STEEL Welding

AISI 9310 alloy steel has good weldability characteristics as it can be welded by a standard process along with the usage of established welding methods.

 

AISI 9310 STEEL Forming

AISI 9310 alloy steel can be readily formed by conventional procedures as this steel has good ductility even in the tempered and quenched condition.

 

AISI 9310 STEEL Machinability

AISI 9310 alloy steel can be machined by conventional methods and good results are obtained when this alloy steel is machined in the tempered or annealed condition.

 

AISI 9310 STEEL Hardening

AISI 9310 alloy steel can be hardened by cold working or by thermal treatment and oil quenching.

About Us

Founded in 1998, FuShun covers an area of 3000 square meters, annual sales volume of 20000 tons. We are engaged in the manufacture and export of Tool Steel, Nickel Alloy, Stainless Steel and other special steel products…,View more content About Me.

Contact Lists

General Manager: Ms. Florence

info@fushunspecialsteel.com

Get A Free Quote!

Find your steel grade and get a quote today.

NOW Send Your Inquiry To : info@fushunspecialsteel.com

x