manufacturer of nickel alloy, stainless steel, tool steel, alloy steel

Bimetal Band Saw Blade

FUSHUN SPECIAL STEEL · Blade · Bimetal Band Saw

A bimetal band saw blade is a spring-steel strip with a high-speed steel edge welded to it. The edge grade sets what it can cut, the tooth pitch sets how it cuts it, and the running-in procedure decides how long it lasts. Most blade complaints trace back to the pitch, not to the steel.

0.65–1.6 mm
Backing thickness
65–67 HRC
Edge hardness
13–41 mm
Blade width
M42 / M51 / M2
Edge grades

Bimetal band saw blade: How the Families Differ

The blade is a composite, and the two halves do different jobs. The backing strip is a low-alloy spring steel, hardened and tempered to about 45 HRC so that it survives the tension and the bending fatigue of running around the wheels. The edge is a high-speed steel — M42 with 8 % cobalt, or M51 with more — electron-beam welded to the strip and hardened to 65–67 HRC.

Selection runs in a fixed order. First the material: aluminium and non-ferrous need a coarse pitch and a different tooth form; carbon steel and tool steel take a standard pitch; stainless and nickel alloys work-harden and need a finer pitch and a lower speed. Then the section thickness, which sets the number of teeth in the cut — two to three is the target, never fewer than one.

Bimetal band saw blade is a cutting tool, and it is judged by the cut: the tooth geometry, the grade of the cutting edge and the running-in procedure decide the life far more than the blade body does. A bimetal blade is a strip of spring steel with a high-speed steel edge electron-beam welded to it.

The edge grade sets what the blade can cut. M42 holds hardness at temperature for stainless and tool steel; M51 with more cobalt holds it further; a carbide-tooth blade cuts hardened steel but is brittle under shock. The backing strip sets the fatigue life, and the tooth pitch sets the chip load.

The Two Mistakes That Keep Coming Back

Running a coarse pitch on a thin wall: the teeth straddle the section, the chip load per tooth doubles and the teeth strip.

Taking a new blade straight to production feed. The micro-edge has to be run in at half feed for the first fifty cuts, or it breaks down before it ever reaches its life.

What buyers get wrong
  • Choosing a pitch that puts more than one tooth in the cut on a thin section; the teeth strip.
  • Running a new blade at full feed; the micro-edge breaks down before it has been run in.
  • Using a coolant that attacks the weld line; the bimetal joint is the first place to fail.
  • Comparing blades on price per blade rather than cost per cut; the difference in life is larger than the difference in price.

Selection Matrix

Table 1 — Tooth pitch against the material being cut

Material 3/4 4/6 5/8 6 10/14
Aluminium, non-ferrous Recommended Usable Avoid Avoid Avoid
Carbon steel, 100–250 mm Usable Recommended Usable Avoid Avoid
Tool steel, 20–100 mm Avoid Usable Recommended Usable Avoid
Stainless, 20–100 mm Avoid Avoid Usable Recommended Usable
Thin wall, tube Avoid Avoid Avoid Usable Recommended

Read it as a starting point: the machine, the coolant and the bundle all move the answer by one column.

Grades We Supply

The grades below are the ones we roll and cut most often. Each one is a different compromise on the same three axes — hardenability, toughness and cost — and the last column says which duty each was designed for.

Table 2 — Grades supplied, with the duty each one covers

Edge grade Composition Edge hardness Duty
M2 6 % W, 5 % Mo, 4 % Cr, 2 % V 64–66 HRC Carbon steel, aluminium, general
M42 8 % Co, 9.5 % Mo, 3.75 % Cr 65–67 HRC Stainless, tool steel, Inconel
M51 9.5 % Co, 10 % Mo 66–68 HRC Hard stainless, heat-resistant alloys
Carbide tooth Tungsten carbide tips — Hardened steel above 45 HRC
Bimetal band saw blade — Tooth pitch against section
Figure 1 — Bimetal band saw blade — Teeth per inch for the section being cut

Supply Range and Tolerances

Supply is quoted by length, width, pitch and edge grade. Coils and welded loops are both available.

Table 3 — Supply range and tolerances

Item Range
Width × thickness 13 × 0.65, 19 × 0.9, 27 × 0.9, 34 × 1.1, 41 × 1.3 mm
Tooth pitch 0.75/1.2 to 3/4 TPI, constant or variable
Coil length 30–100 m
Welded loop To the machine length, welded and annealed
Edge grade M2, M42, M51, carbide

Blades are supplied as coils or as welded loops cut to the machine length. The loop is welded, annealed and tensioned; the weld is marked so that it can be run outside the cut.

Properties That Decide the Choice

The blade is a composite: edge hardness, backing tensile and weld strength are three separate properties and are tested separately.

Table 4 — Properties that decide the selection

Property Value Test
Edge hardness 65–67 HRC HV converted, 3 points
Backing hardness 44–48 HRC HV converted
Backing tensile ≥1,200 MPa Strip tensile
Weld shear strength ≥650 MPa Weld shear test
Fatigue ≥1 × 10⁶ cycles at 300 MPa Bending fatigue

Chemical Composition

The edge is a high-speed steel with cobalt and molybdenum for hot hardness; the backing strip is a spring steel with the fatigue resistance to survive the tension.

Table 5 — Chemical composition, wt. %

Grade C Si Mn Cr Mo Ni V
M42 1.05–1.15 ≤0.65 ≤0.40 3.50–4.25 9.00–10.00 — 1.00–1.40
M51 1.20–1.30 ≤0.65 ≤0.40 3.80–4.50 9.00–10.50 — 1.20–1.60
M2 0.78–0.88 ≤0.45 ≤0.40 3.75–4.50 4.50–5.50 5.50–6.75 1.75–2.20

Heat Treatment

The edge is hardened and tempered before the weld; the weld zone is then annealed so that the backing strip does not become brittle.

Table 6 — Heat treatment schedule

Step Temperature Time / atmosphere Cooling
Edge hardening 1,180–1,220 °C Austenitise, quench Salt or vacuum
Edge tempering 540–560 °C 2 h, twice Air
Weld annealing 700–760 °C Local, 10–20 s Air
Backing hardening 850–880 °C Quench and temper to 45 HRC Oil
Bimetal band saw blade — Blade life against running-in feed
Figure 2 — Bimetal band saw blade — Relative life of an M42 blade, 304 stainless, 100 mm bar

How These Grades Fail

Blades fail at the tooth root. The crack starts where the tooth meets the backing, propagates through the backing and the blade breaks across the width. That is a fatigue failure driven by the bending cycle around the wheels — which is why the wheel diameter has a minimum for each blade width.

The second failure is edge chipping. Stainless and nickel alloys work-harden under the tooth; a blade that rubs instead of cutting will chip within a few cuts, and the chips grow into a strip.

Certificate and Testing

  • EN 10204 3.1 mill certificate with chemistry and mechanical properties, heat number and melt route.
  • Hardness survey and dimensional report on every piece on request.
  • Ultrasonic inspection to ASTM A388 or SEP 1921 where the section or the application calls for it.
  • Third-party inspection — SGS, BV, TUV — arranged before dispatch, at the customer’s instruction.
  • Spectro check on the finished part where a weld or a heat treatment has been added after despatch.

Packing, MOQ and Delivery Terms

Coils are packed in a cardboard sleeve with the tooth pitch and grade on the label; loops are coiled and boxed. Blades are oiled for sea freight.

Table 7 — Trade terms, packing and documents

Item Standard terms
Trade terms FOB Shanghai / CIF / CFR / EXW; FOB is the default.
Minimum order One bundle, plate or coil for stock sizes; mill runs quoted individually.
Lead time 20–30 days from order confirmation for stock sizes; 30–45 days where forging or heat treatment is included.
Payment 30 % T/T deposit, 70 % against the bill of lading copy; L/C at sight above 20 t.
Packing Seaworthy export packing — crated or strapped, marked with grade, heat number, size and net weight.
Documents EN 10204 3.1 certificate, packing list, invoice, bill of lading, certificate of origin; legalisation on request.

Frequently Asked Questions

What tooth pitch should I use?

Two to three teeth in the cut. A 100 mm solid bar takes a 4/6 pitch; a 10 mm wall takes 10/14. The matrix above gives the starting point.

Which edge grade cuts stainless?

M42 or M51, at a lower surface speed than carbon steel. M2 will cut it but the life is shorter.

How do I run in a new blade?

Half feed and half speed for the first fifty cuts, then step up over the next hundred.

Can you weld loops to length?

Yes, to the machine length, welded and annealed, with the weld marked.

Do you supply carbide-tooth blades?

For hardened steel above 45 HRC, yes, quoted against the section and the machine.

Bimetal band saw blade coil with M42 edge
Figure 3 — Bimetal band saw blade, M42 edge on a spring-steel backing

Related Grades

Browse the full range: blade grades.

Request a Quote

Five lines are enough to quote
  • Grade and governing standard
  • Form, size and quantity
  • Delivery condition and hardness
  • Certificate and testing requirements
  • Destination port and required date

Email [email protected] or use the form below. Drawings in DXF, STEP or PDF are all fine. Stock sizes ship within 20 days of order confirmation.

About Us

Founded in 1998, FuShun covers an area of 3000 square meters, annual sales volume of 20000 tons. We are engaged in the manufacture and export of Tool Steel, Nickel Alloy, Stainless Steel and other special steel products…,View more content About Me.

Contact Lists

General Manager: Ms. Florence

[email protected]

Get A Free Quote!

Find your steel grade and get a quote today.

NOW Send Your Inquiry To : [email protected]

x