manufacturer of nickel alloy, stainless steel, tool steel, alloy steel

M2 High Speed Steel Heat Treatment Analysis

M2 High Speed Steel Heat Treatment Analysis

 

M2 High Speed Steel Preheating

To minimize distortion and stresses in large or complex tools use a double preheat. Heat at a rate not exceeding 400°F per hour (222°C per hour) to 1100°F (593°C) equalize, then heat to 1450-1550°F (788-843°C). For normal tools, use only the second temperature range as a single preheating treatment

 

M2 High Speed Steel Austenizing(High Heat)

Heat rapidly from the preheat.

For Cutting Tools:

Furnace: 2200-2250°F (1204-1232°C)

Salt: 2175-2225°F (1191-1218°C)

To maximize toughness, use the lowest temperature. To maximize hot hardness, use the highest temperature.

For punches, dies, and tools that require maximum toughness without hot hardness:

Furnace: 2075-2175°F (1175-1191°C)

Salt: 2050-2150°F (1121-1177°C)

 

M2 High Speed Steel Quenching

Pressurized gas, warm oil, or salt. For pressurized gas, a rapid quench rate to below 1000°F (538°C) is critical to achieve the desired properties. For oil, quench until black, about 900°F (482°C), then cool in still air to 150-125°F (66-51°C). For salt maintained at 1000-1100°F (538-593°C), equalize, then cool in still air to 150-125°F (66-51°C).

 

M2 High Speed Steel Tempering

Temper immediately after quenching. Typical tempering range is 1025-1050°F (552-566°C). Hold at temperature for 2 hours, then air cool to ambient temperature. Double tempering is required. For large cross sections, and especially for blanks from which tools will be cut by wire EDM, triple tempering is strongly recommended.

 

M2 High Speed Steel Hardening Temperature,°F

Double Tempering Temperature,°F 2150 2200 2225
800 61HRC 61.5HRC 62HRC
850 61.5HRC 62HRC 62.5HRC
900 62.5HRC 63HRC 63.5HRC
950 63HRC 64HRC 65HRC
1000 64HRC 65HRC 65.5HRC
1025 63.5HRC 65HRC 65.5HRC
1050 63HRC 64.5HRC 65HRC
1100 61.5HRC 62.5HRC 63.5HRC
1150 57.5HRC 59HRC 60HRC
1200 51HRC 54HRC 55HRC

 

M2 High Speed Steel Annealing

Annealing must be performed after hot working and before re-hardening

Heat at a rate not exceeding 400°F per hour (222°C per hour) to 1525-1550°F (829-843°C), and hold at temperature for 1 hour per inch (25.4 mm) of thickness, 2 hours minimum. Then cool slowly with the furnace at a rate not exceeding 50°F per hour (28°C per hour) to 1000°F (538°C). Continue cooling to ambient temperature in the furnace or in air.

 

M2 High Speed Steel Forging

Pre heat slowly to 850 – 900°C, then increase more quickly to the forging temperature of 1050 – 1150°C. Do not forge below 880 – 900°C. Cool very slowly after forging. If during the forging the temperature of the M2 high speed tool steel material drops below 880-900°C, re-heating will be necessary. Cool the M2 steel component very slowly after forging.

 

M2 High Speed Steel Harden

Heat slowly to 1550° F, soak thoroughly, heat to 1850° F, soak thoroughly. Soak time in the furnace varies from a few minutes to 15 minutes, depending tool size, heat capacity of the furnace, and the size of the charge. – Heat to 2150 to 2200° F for max. toughness and minimum distortion. – Heat to 2250 to 2275° F for max. hardness and abrasion resistance.

 

M2 High Speed Steel Heat Treating

ANNEALING PREHEAT AUSTENITIZING QUENCH TEMPERING
Temp Temp Temp Medium Temp
°F °F °F   °F
1550/1600 1500/1550 2175/2225 Salt/Oil/Atm 1025/1050

 

M2 HIGH SPEED STEEL THERMAL EXPANSION

Temperature 10^-6 m/(m*K) 10^-6 in/in °F
°F °C
212 100 11.5 6.5
392 200 11.7 6.6
572 300 12.2 6.9
752 400 12.4 7
932 500 12.7 7.1
1112 600 13 7.3
1292 700 12.9 7.3

 

M2 HIGH SPEED STEEL MECHANICAL PROPERTY

Hardness, Rockwell C (tempered at 620°C, quenched at 1200°C) 62
Hardness, Rockwell C (as hardened, quenched at 1200°C) 65
Compressive yield strength (when tempered at 150°C) 3250 MPa
Izod impact unnotched (when tempered at 150°C) 67 J
Abrasion (loss in mm 3 , as-hardened; ASTM G65) 25.8
Abrasion (loss in mm 3 , tempered at 690°C; ASTM G65) 77.7
Poisson’s ratio 0.27-0.30
Elastic modulus 190-210 GPa

Fushun Special Steel LTD CO

Fushun Metal is a large special steel manufacuter and supplie. We are metal experts and have been providing quality customer service and products since 1998.

 

At Fushun Metal, we supply a wide range of metals for a variety of applications. Our products/stock includes: stainless steel, alloy steel, spring steel, tool steel, high speed steel, mould steel, nickel alloy.

 

Our hot rolled and cold rolled steel is available in a wide range of shapes including: bars, tubes, sheets and plates. We can cut metal to your exact specifications.

 

Send your inquiry information to us and get a free quotation today!

About Us

Founded in 1998, FuShun covers an area of 3000 square meters, annual sales volume of 20000 tons. We are engaged in the manufacture and export of Tool Steel, Nickel Alloy, Stainless Steel and other special steel products…,View more content About Me.

Contact Lists

General Manager: Ms. Florence

[email protected]

Get A Free Quote!

Find your steel grade and get a quote today.

NOW Send Your Inquiry To : [email protected]

x