HS3-3-2, 1.3333, High-speed Tool Steel

HS3–3–2,1.3333, High-speed Tool Steel

HS3-3-2, 1.3333, High-speed Tool Steel

Designation by Standards

 

Mat. No. EN
1.3333 HS3-3-2

 

Chemical Composition (in weight %)

 

C Si Mn P S Cr Mo W V
0.95 – 1.03 max 0.45 max 0.4 max 0.03 max 0.03 3.8 – 4.5 2.5 – 2.9 2.7 – 3 2.2 – 2.5

 

Description

Economical high speed steel for medium life times. The steel has high toughness properties and is suitable for tools which are exposed to knocks and bumps.

 

Applications

In the metal plating sector, metal circular saw blades, long saw blades and blades for wood machining are manufactured from this steel as a matter of preference.

 

Physical properties (average values) at ambient temperature

Modulus of elasticity [103 x N/mm2]: 210

Density [g/cm3]: 8.0

Thermal conductivity [W/m. K]: 20.0

Electric resistivity [Ohm mm2/m]: 0.65

Specific heat capacity[J/g. K]: 0.46

Soft Annealing

Heat to 780-820oC, cool slowly in furnace. This will produce a maximum Brinell hardness of 255.

Stress Relieving

Stress relieving to remove machining stresses should be carried out by heating to 600-650oC, holding for one hour at heat, followed by air cooling. This operation is performed to reduce distortion during heat treatment.

Hardening

Harden from a temperature of 1170- 1220oC followed by oil or air quenching or warm bath 550-220oC.

Tempering

Tempering temperature: 520-550oC, at least 2x for at least 62 HRC.

Forging

Hot forming temperature: 1150-900oC.

 

About Us

Founded in 1998, FuShun covers an area of 3000 square meters, annual sales volume of 20000 tons. We are engaged in the manufacture and export of Tool Steel, Nickel Alloy, Stainless Steel and other special steel products…,View more content About Me.

Contact Lists

General Manager: Ms. Florence

[email protected]

Get A Free Quote!

Find your steel grade and get a quote today.

NOW Send Your Inquiry To : [email protected]

x