manufacturer of nickel alloy, stainless steel, tool steel, alloy steel

Stainless Steel Surface Finish Types: The Four Standards, One Table

Stainless Steel Surface Finish Types: The Four Standards, One Table

GB, ASTM, EN and JIS describe the same eight surfaces with four different code systems. This page puts them side by side, gives the roughness each one actually delivers, and shows what to write on the order so the mill cannot choose for you.

A surface finish code is not a cosmetic instruction. It fixes three things at once: the arithmetic mean roughness the sheet will measure, the defects that are permitted on the face, and whether the surface is still in its passivated state. Two sheets with the same code from two mills can differ by a factor of three in roughness and still both be “correct”, because the standard controls the process route rather than a single number.

That is why procurement arguments about finish are so common and so unproductive. The fix is to quote the standard, the code and the roughness limit together — and to know which codes are equivalent across the four systems and which are merely similar.

What the code actually constrains

  • Roughness — the arithmetic mean Ra over the measured length. This is the number that decides cleanability, friction and how visible a fingerprint is.
  • Defects — each standard defines the permitted size and count of scratches, pits, roll marks, inclusions and edge defects for that route. A 2B sheet is allowed roll marks; a No.4 sheet is not allowed a scratch deeper than the grain it was produced with.
  • Passivation state — a pickled or bright annealed surface carries a chromium oxide film formed in the mill. A mechanically polished surface carries a film formed in air afterwards, which is thinner and less uniform. This is why polishing a 2B sheet does not automatically improve its corrosion resistance.

The four systems, side by side

The table maps the eight surfaces that account for almost all tonnage. Where a standard has no exact equivalent, the nearest code is given with a note.

Table 1. Surface finish codes across GB, ASTM, EN and JIS, with the route each one describes.

Surface Process route GB/T 3280 ASTM A480 EN 10088-2 JIS G4305
Hot rolled, pickled Hot rolled, annealed, pickled No.1 No.1 1D No.1
Cold rolled, matte Cold rolled, annealed, pickled 2D No.2D 2D No.2D
Cold rolled, bright Cold rolled, annealed, pickled, skin passed 2B No.2B 2B No.2B
Bright annealed Cold rolled, bright annealed in H2/N2 BA No.2BA 2R BA
Coarse ground Ground with 80–120 grit No.3 No.3 2G No.3
Brushed Polished with 150–180 grit, non-directional No.4 No.4 2J No.4
Hairline Continuous linear grain, 150–320 grit HL No.4 (HL) 2K HL
Mirror Progressive polishing to 0.01–0.05 µm No.8 No.8 2Q No.8

Two mismatches are worth flagging. First, EN 2J and 2K split what ASTM and JIS call No.4 and HL into a dull polished and a satin finish; a European drawing that says 2K is asking for a directional grain, which is closer to HL than to No.4. Second, ASTM No.5 exists but is rarely ordered — it sits between No.4 and No.6 and most mills will quote No.6 instead.

Roughness: what each finish actually measures

The codes describe a route, not a number. The chart below gives the range actually measured on production sheet, which is wider than most catalogues suggest.

Range chart of surface roughness Ra for BA, No.8 mirror, 2B, HL, 2D, No.4, No.3 and 1D stainless finishes on a log scale
Figure 1: The overlaps are real. A 2B and a No.4 can measure the same Ra and look completely different, because one is a rolled surface and the other is a cut surface.

Table 2. Typical roughness and where each finish is used.

Surface Typical Ra Corrosion behaviour Typical application
1D 1.0–3.0 µm Good; oxide intact Process vessels, structural plate, heat exchanger shells
2D 0.4–1.0 µm Good; oxide intact Deep drawn parts, automotive, further processing
2B 0.1–0.5 µm Good; standard reference surface Kitchen equipment, appliances, general fabrication
BA 0.03–0.2 µm Best of the mill finishes Hygienic equipment, pharmaceutical, tube
No.4 0.4–1.0 µm Slightly reduced; oxide reformed in air Restaurant equipment, architectural trim, lifts
HL 0.2–0.8 µm Slightly reduced; grain traps residue Elevator panels, facades, appliance fronts
No.8 0.01–0.05 µm Variable; depends on polishing residue Decorative panels, mirrors, press plates

The counter-intuitive part

A mirror finish is not the most corrosion resistant finish. Polishing removes the mill oxide and leaves a surface that re-passivates in air, and any polishing compound trapped in a scratch becomes a corrosion initiation site. For a marine or hygienic application, 2B or BA outperforms No.8 at a lower cost.

Thickness decides which finishes you can buy

The surface codes are tied to the rolling route, and the rolling route is tied to thickness. This is the constraint that catches buyers who specify a finish from a catalogue picture without checking the size.

Chart of available stainless surface finishes by thickness, showing cold rolled finishes up to 3 mm and hot rolled finishes above
Figure 2: Above 3 mm the cold rolled finishes disappear. A drawing that asks for 2B in 10 mm plate is asking for a product that does not exist.

Six finishes, and what each one costs you

  • 2B — the default. Cheapest, widest availability, best formability because the skin pass is light. If a drawing does not specify a finish, this is what arrives; the rolling route behind it explains why the same code is not available in 10 mm plate.
  • 2D — rougher than 2B and better for drawing because the surface holds lubricant. Choose it when the part is formed, not when it is seen.
  • BA — brighter than 2B and produced without pickling, so the surface is free of the acid attack that can leave a smut. It carries a price premium of 5–12 % and a much longer lead time in some sizes.
  • No.4 — the workhorse decorative finish. It hides fingerprints and small handling marks, which is why it dominates commercial kitchens. It cannot be repaired locally: a scratch has to be re-grained across the whole panel.
  • HL — directional and cheaper to produce than a full No.4 because the grain is continuous. It shows scratches parallel to the grain and hides them across it, which is exactly the opposite of what most people expect.
  • No.8 — the most expensive and the least forgiving. A 0.5 mm sheet polished to No.8 will show every deflection as a distortion of the reflected image, so the flatness specification matters as much as the roughness.

What to put on the purchase order

Six lines close the gap between what the buyer means and what the mill ships:

  • Standard, grade and finish code — for example ASTM A240 Type 304, finish No.4, ASTM A480. Naming only “No.4” is not a specification. The 304 grade page lists the product forms each finish is stocked in.
  • Roughness limit if the finish is functional — for example Ra 0.8 µm maximum. This converts a process description into a measurable acceptance criterion.
  • Thickness and width, because the available finish depends on both.
  • Which face is finished. Cold rolled sheet is finished on both faces; plate is often finished on one, and the other may be as-rolled.
  • Protection — interleaved paper, laser film or PVC. A No.4 or No.8 surface that arrives scratched has lost the premium that was paid for it.
  • Certificate — EN 10204 3.1, with the finish code and, where specified, the roughness result on the test certificate.

Four arguments that come up on inspection

“This is not No.4.” No.4 is defined by the abrasive grit range, not by an appearance. A 150-grit and a 180-grit finish look different and both are No.4. If the appearance matters, specify the grit or the Ra.

“The BA is not bright enough.” Brightness depends on the annealing atmosphere and on whether the sheet was skin passed. EN 2R and JIS BA are not identical for this reason; ask for the gloss value if the part is visible.

“There are scratches under the film.” Handling scratches within the permitted depth are not a defect on a 2B sheet. On a No.8 sheet they are. The standard defines the limit per finish, which is why the finish code has to be on the drawing.

Edge condition is part of the same argument. A No.4 face with a rolled-over burr on the cut edge will rust at the edge first, which is why deburring and edge breaking belong in the surface specification rather than in a separate note.

“The polished part rusted.” Almost always a residue problem, not a steel problem. Polishing compound or iron contamination from a carbon steel brush sits in the grain and initiates corrosion. Pickling and passivation after fabrication is the answer, not a different grade.

Frequently asked questions

What is the difference between 2B and BA finish?

Both are cold rolled and annealed. 2B is pickled and then skin passed, which leaves a light grey semi-reflective surface. BA is annealed in a hydrogen-nitrogen atmosphere instead of being pickled, which leaves a brighter, smoother surface with a thinner oxide. BA costs more and is harder to source in heavy thickness.

Which finish is best for corrosion resistance?

Among mill finishes, BA and 2B are the reference surfaces: the oxide is intact and uniform. No.4 and HL remove part of that oxide mechanically and rely on re-passivation in air. The worst choice for corrosion is a mirror polish with polishing residue left in the grain.

Can 2B be polished to No.4 later?

Yes, and it is common. The risk is that the polishing is done without a final passivation step, and the surface ends up with embedded iron. If the part is going into a food or marine environment, specify passivation after polishing.

Is HL the same as No.4?

No. Both are mechanical finishes, but No.4 is non-directional and HL has a continuous linear grain. ASTM does not have a separate HL code and describes it under No.4; EN uses 2K and JIS uses HL.

What thickness can be supplied in No.8?

Typically 0.3–1.5 mm in cold rolled sheet. Above that, polishing a thick plate to a mirror finish is possible but the flatness requirement becomes the limiting factor, and the part usually has to be polished after forming rather than before.

Related reading

Fushun Metal · ISO 9001 · AS9120B
Send the grade, size and standard.

You get chemical composition, mechanical properties and a price — with inspection certificates to EN 10204 3.1 issued against the heat number.

Request a quoteWhatsApp +86 178 7358 1838

[email protected]  ·  +86 731 8990 3933

About Us

Founded in 1998, FuShun covers an area of 3000 square meters, annual sales volume of 20000 tons. We are engaged in the manufacture and export of Tool Steel, Nickel Alloy, Stainless Steel and other special steel products…,View more content About Me.

Contact Lists

General Manager: Ms. Florence

[email protected]

Get A Free Quote!

Find your steel grade and get a quote today.

NOW Send Your Inquiry To : [email protected]

x