IN718 / GH4169 Atomization Rod for PREP, VIGA and EIGA

Master alloy · Atomization rod · GH4169 / N07718

IN718 / GH4169 Atomization Rod, Built to Your Atomizer

An electrode, not a length of bar. GH4169 rod for powder production is judged by whether it fits the clamp, whether the nose seats, whether the surface is clean enough to keep oxygen out of the melt, and whether the heat number can still be read after the first run. We machine it to Ø30–130 mm, Ra ≤1.6 µm, with the EIGA 70° nose and the end-face marking the standards require.

Ø30–130 mm
Rod diameter
Ra ≤1.6 µm
Ground surface
70°
EIGA nose angle
O ≤30 ppm
Atomization grade

At a glance

Item GH4169 atomization rod
Designation GH4169 · IN718 · UNS N07718 · W.Nr 2.4668
Form Round rod, straight lengths, ends machined; centre hole or thread on request
Size Ø30–130 mm, length 120–700 mm or cut to the clamp length
Condition Black, turned, ground, or mirror polished; Ra ≤1.6 µm for PREP and EIGA
Melting route VIM+VAR or VIM+ESR+VAR; single VIM only below 30 ppm by agreement
Standards GB/T 38941 (PREP sizes) · AMS 5383 chemistry · customer drawing
Marking Grade, final melt heat number and melt date stamped on the end face

This page covers the rod. It does not cover the powder: we sell the electrode, and the atomizer turns it into powder. That boundary is worth keeping in mind, because most arguments about “powder quality” start with an electrode that was ordered without a drawing.

Why a rod is not a bar

A bar is ordered by diameter and grade. A rod is ordered against a machine. The same Ø80 mm section can be wrong for three different atomizers because the clamp length, the nose angle and the surface finish all come from the equipment, not from the alloy.

Atomizer Diameter Diameter tolerance Length End geometry Surface
PREP Ø30–100 mm ±2 mm Per clamp Flat, chamfered Ra ≤1.6 µm
VIGA Ø50–130 mm ±1 mm Per clamp Flat, centre hole optional Turned or ground
EIGA Ø50–100 mm ±1 mm Per clamp 70° cone on one end Ra ≤1.6 µm

Two details decide whether the first run works. The centre hole, if there is one, must be free of coolant and oil — a drilled hole that is never cleaned is a virtual leak in the chamber. And the straightness has to survive the clamp: a rod that is straight on the bench but spring-loaded in the fixture will run out of concentricity and spray unevenly.

Atomization rod end geometries for PREP, VIGA and EIGA atomizers
The three end geometries we machine most often: flat with chamfer for PREP, flat with an optional centre hole for VIGA, and the 70° cone required on EIGA electrodes.

Chemical composition

Element, % GH4169 (GB/T 14992) IN718 (AMS 5383)
C ≤0.08 ≤0.08
Cr 17.0–21.0 17.0–21.0
Ni 50.0–55.0 50.0–55.0
Mo 2.8–3.3 2.8–3.3
Nb+Ta 4.75–5.50 4.75–5.50
Ti 0.65–1.15 0.65–1.15
Al 0.20–0.80 0.20–0.80
Co ≤1.00 ≤1.00
B ≤0.006 ≤0.006
Si / Mn ≤0.35 / ≤0.35 ≤0.35 / ≤0.35
P / S ≤0.015 / ≤0.015 ≤0.015 / ≤0.015
Fe Balance Balance

The two windows are the same. What differs is the sampling and retest discipline behind them, and for atomization the more useful conversation is about Nb: it segregates in the ingot, and a rod cut from the segregated end will not atomize into the same powder as one cut from the middle. If the powder is for a rotating part, ask where along the ingot the rod was taken.

Gas and inclusion limits

Item Atomization grade General bar grade
Oxygen ≤30 ppm (20 ppm on request) 30–50 ppm
Nitrogen ≤30 ppm ≤50 ppm
Sulphur ≤15 ppm ≤15 ppm
Trace elements Per AMS 2280, report per heat On request
Inclusion rating Metallographic report, agreed scale Not normally specified
Surface contamination No oil, no coolant residue, no grinding burn —

Oxygen in the rod is the floor for oxygen in the powder; atomization only adds to it. A heat at 40 ppm will not produce a 15 ppm powder no matter how good the atomizer is, which is why the rod specification should be written backwards from the powder specification.

What the consolidated powder has to hit

Property 20 °C 650 °C
Tensile strength, MPa ≥1276 ≥1000
0.2 % yield, MPa ≥1034 ≥862
Elongation, % ≥12 ≥12
Reduction of area, % ≥15 ≥15

These are the AMS 5662 values for wrought IN718, quoted as the reference the customer’s part is usually judged against after HIP and heat treatment. They are not properties of the rod and we do not test them on the rod: the acceptance route for an electrode is chemistry, gas, density, geometry and surface. Anyone offering you tensile data measured on an atomization rod is selling something else.

Melting route and standards

Route Oxygen Relative cost Fits
VIM only 30–50 ppm 1.0 Industrial powder, cladding, non-rotating parts
VIM + VAR 20–30 ppm 1.3–1.6 LPBF and EIGA stock for structural parts
VIM + ESR + VAR ≤10–15 ppm 1.6–2.0 Rotating parts, aerospace powder

For a rotating part the route is normally triple melt and the drawing says so. For a laser-cladding or cold-spray grade, single VIM at a controlled oxygen level is the economic answer. The mistake is to buy the triple-melt route for a part that will never be audited, or to buy single melt for one that will.

Sizes follow GB/T 38941 for PREP, and the VIGA and EIGA geometries in the revision now in circulation. Where the two disagree, the customer’s clamp drawing wins — and we machine to it rather than to the nearest standard size.

End-face marking, packing and traceability

  • Stamped on the end face — grade, final melt heat number, melt date; a fourth line for the rod serial if the customer asks
  • Marking method — low-stress stamp or laser, clear of the seat and the clamp zone
  • Packing — individual sleeve, VCI paper, crate with desiccant; ends protected against nicks
  • Documents — EN 10204 3.1 with chemistry and gas, dimensional report, surface roughness record

The marking requirement is not decorative. If the heat number cannot be read when the rod comes back out of the atomizer, the powder lot loses its link to the melt, and that link is the whole point of buying master alloy rather than scrap.

What to send with an enquiry

Send these five lines and we quote within one working day
  • Atomizer make and model, or the clamp drawing
  • Rod diameter, length and single weight, with tolerance
  • End geometry — flat, centre hole, 70° cone, thread
  • Surface requirement — turned, ground, Ra value
  • Oxygen limit and acceptance standard, plus the powder specification it has to serve

Email [email protected]  ·  WhatsApp +86 178 7358 1838  ·  or use the form below.

FUSHUN METAL · AS9120B · EN 10204 3.1 with the heat number.

Related forms and grades

The same heat, in the form the next operation needs.

About Us

Founded in 1998, FuShun covers an area of 3000 square meters, annual sales volume of 20000 tons. We are engaged in the manufacture and export of Tool Steel, Nickel Alloy, Stainless Steel and other special steel products…,View more content About Me.

Contact Lists

General Manager: Ms. Florence

[email protected]

Get A Free Quote!

Find your steel grade and get a quote today.

NOW Send Your Inquiry To : [email protected]

x