manufacturer of nickel alloy, stainless steel, tool steel, alloy steel

1.7711, 40CrMoV4-6, Creep-Resisting Steel

1.7711 40CrMoV4-6 Steel

40CrMoV4-6 DIN 1.7711 Alloyed Carbon Steel

1.7711 40CrMoV4-6 DIN Steel

40CrMoV4-6 Creep-Resisting Steel (EN 10269, DIN 1.7711)

Product Description

FUSHUN METAL’s 40CrMoV4-6 (1.7711) is a premium chromium-molybdenum-vanadium creep-resisting steel offering an exceptional combination of high temperature strength, excellent creep resistance, good toughness, and superior long-term durability at elevated temperatures. With a carefully engineered chemical composition featuring optimized levels of chromium (0.90-1.20%), molybdenum (0.50-0.65%), and vanadium (0.25-0.35%), our 40CrMoV4-6 delivers outstanding performance in demanding applications requiring mechanical strength at high temperatures up to 550°C. Available in multiple forms including round bars, flat bars, plates, forgings, and custom shapes, this versatile steel is ideal for applications in high-temperature fasteners, steam turbine components, pressure vessel parts, power generation equipment, and other applications where long-term performance at elevated temperatures is essential. The balanced alloy content provides excellent hardenability combined with exceptional creep rupture strength and high-temperature stability. Each product undergoes comprehensive quality control to ensure consistent properties, precise dimensions, and superior surface quality for reliable performance in critical high-temperature industrial applications.

Equivalent Steel Grades

40CrMoV4-6 (1.7711) is part of a family of creep-resisting steels with the following equivalent grades in different standards:

Standard Designation Comparable Grades
Europe / EN 40CrMoV4-6 30CrMoV9, 34CrMo4, 25CrMo4
Germany / DIN 1.7711 / 40CrMoV4-6 1.7707 (30CrMoV9), 1.7220 (34CrMo4)
Italy / UNI 40CrMoV4-6 38CrMoV5.2, 35CrMo4
France / AFNOR 40CrMoV4-6 35CD4, 30CD12
UK / BS 670-860 708M40, 708A37
USA / ASTM A193 B16 A193 B7, 4140 (modified)
China / GB 40CrMoV4-6 35CrMo, 42CrMo

Chemical Composition

FUSHUN METAL’s 40CrMoV4-6 (1.7711) Steel features the following chemical composition according to EN 10269:2013 standard:

Element Content (%) Allowed Product Deviations
Carbon (C) 0.36-0.44% ±0.02
Silicon (Si) 0.40% max +0.03
Manganese (Mn) 0.45-0.85% ±0.04
Phosphorus (P) 0.025% max +0.005
Sulfur (S) 0.030% max +0.005
Chromium (Cr) 0.90-1.20% ±0.05
Molybdenum (Mo) 0.50-0.65% ±0.03
Vanadium (V) 0.25-0.35% ±0.03
Aluminum (Al) total 0.015% max ±0.05
Iron (Fe) Balance

Key Element Functions

  • Carbon (0.36-0.44%): Provides optimum hardness and strength after heat treatment. The moderate carbon content ensures good toughness while enabling adequate hardness.
  • Chromium (0.90-1.20%): Enhances hardenability, provides oxidation resistance at elevated temperatures, and improves creep resistance. The chromium content also contributes to good hot strength.
  • Molybdenum (0.50-0.65%): Significantly improves creep resistance, high-temperature strength, and thermal stability. Molybdenum is essential for long-term performance at elevated temperatures.
  • Vanadium (0.25-0.35%): Forms stable vanadium carbides that refine grain size, enhance high-temperature strength, and improve creep resistance. Vanadium also contributes to tempering resistance.
  • Manganese (0.45-0.85%): Enhances hardenability and contributes to overall strength.
  • Silicon (max 0.40%): Contributes to deoxidation during steelmaking and improves oxidation resistance at elevated temperatures.

Available Product Forms and Dimensions

FUSHUN METAL offers 40CrMoV4-6 (1.7711) Creep-Resisting Steel in a wide range of forms to meet diverse application requirements:

Round Bar Specifications

Diameter (mm) Standard Length (mm) Tolerance Surface Condition
10 – 25 3000, 6000, Fixed or Random h9, h10, h11, k12 Black, Peeled, Turned, Ground, Polished
26 – 100 3000, 6000, Fixed or Random h9, h10, h11, k12 Black, Peeled, Turned, Ground, Polished
102 – 160 3000, 6000, Fixed or Random h9, h10, h11, k12 Black, Peeled, Turned, Ground
162 – 300 2000, 3000, Fixed or Random h10, h11, k12 Black, Peeled, Turned, Rough Ground
305 – 500 1000, 2000, Fixed or Random h11, k12 Black, Peeled, Turned

Flat Bar Specifications

Thickness (mm) Width (mm) Standard Length (mm) Tolerance Surface Condition
5 – 15 20 – 100 3000, 6000, Fixed or Random EN 10278, EN 10058 Hot Rolled, Cold Drawn, Ground
16 – 30 30 – 150 3000, 6000, Fixed or Random EN 10278, EN 10058 Hot Rolled, Cold Drawn, Ground
32 – 50 40 – 200 3000, 6000, Fixed or Random EN 10058 Hot Rolled, Cold Drawn, Ground
55 – 80 60 – 300 3000, 6000, Fixed or Random EN 10058 Hot Rolled, Cold Drawn
85 – 120 80 – 400 3000, Fixed or Random EN 10058 Hot Rolled
125 – 200 100 – 500 2000, 3000, Fixed or Random EN 10058 Hot Rolled

Plate Specifications

Thickness (mm) Width (mm) Length (mm) Tolerance Surface Condition
5 – 10 Up to 2000 Up to 6000 EN 10029, ASTM A6 Hot Rolled, Pickled, Ground
12 – 25 Up to 2500 Up to 8000 EN 10029, ASTM A6 Hot Rolled, Pickled, Ground
30 – 60 Up to 2500 Up to 10000 EN 10029, ASTM A6 Hot Rolled, Pickled
65 – 100 Up to 2200 Up to 8000 EN 10029, ASTM A6 Hot Rolled
110 – 160 Up to 2000 Up to 6000 EN 10029, ASTM A6 Hot Rolled

Square Bar Specifications

Size (mm) Standard Length (mm) Tolerance Surface Condition
10 x 10 – 30 x 30 3000, 6000, Fixed or Random h11, h12, k12 Hot Rolled, Cold Drawn, Ground
35 x 35 – 80 x 80 3000, 6000, Fixed or Random h11, h12, k12 Hot Rolled, Cold Drawn, Ground
85 x 85 – 150 x 150 3000, 6000, Fixed or Random h12, k12 Hot Rolled, Ground
160 x 160 – 300 x 300 2000, 3000, Fixed or Random k12, k13 Hot Rolled

Hexagonal Bar Specifications

Size (mm) Standard Length (mm) Tolerance Surface Condition
10 – 30 (across flats) 3000, 6000, Fixed or Random h11, h12 Hot Rolled, Cold Drawn, Ground
32 – 60 (across flats) 3000, 6000, Fixed or Random h11, h12 Hot Rolled, Cold Drawn, Ground
65 – 100 (across flats) 3000, Fixed or Random h12, k12 Hot Rolled, Cold Drawn

Special Shapes and Custom Dimensions

FUSHUN METAL also offers 40CrMoV4-6 (1.7711) in custom shapes, sizes, and pre-machined conditions to meet specific application requirements:

  • Near-net shape forgings
  • Pre-machined fastener blanks
  • Custom profile sections
  • Pre-machined turbine components
  • Custom mechanical parts
  • Hollow bars and tubes
  • Pre-machined pressure vessel parts
  • Custom forged shapes per drawing

Heat Treatment Conditions

FUSHUN METAL can supply 40CrMoV4-6 (1.7711) in various heat treatment conditions according to EN 10269:2013 standard:

Process Temperature °C Cooling Medium Resulting Hardness
Hot-forming 1100-950
Normalizing (+N) 880-900 Air
Quenching (+Q) 900-970 Oil or polymer
Tempering (+T) 650-720 Air
Stress-relieving (+SR) 50 under the temp. of tempering
Natural state (+U) HB max 350
Soft annealing (+A) 680-730 Air HB max 241
Isothermal annealing (+I) 880 furnace cooling to 730, then air
Spheroidized annealed (+AC) 830 slow furnace cooling HB 220
Quenching and stress-relieving 930 oil, 200 air HRC ~54
Pre-heating welding 300
Stress-relieving after welding 560 furnace cooling

Critical Temperatures

AC1 (°C) AC3 (°C) MS (°C) Mf (°C)
760 870 340 120

Mechanical Properties

40CrMoV4-6 (1.7711) offers excellent mechanical properties for high-temperature applications according to EN 10269:2013 standard:

Mechanical Properties at Room Temperature (Quenched and Tempered Condition)

Size Range (mm) Tensile Strength (N/mm²) Yield Strength Rp0.2 (N/mm²) min. Elongation A (%) min. Reduction of Area Z (%) min. Impact Energy Kv2 (J) min. Hardness (HBW) for information
≤ 100 850-1000 700 14 45 30 253-298
100 – 160 850-1000 640 14 45 25 253-298

Minimum Yield Strength at Elevated Temperatures (EN 10269:2013)

Size Range (mm) 50°C 100°C 150°C 200°C 250°C 300°C 350°C 400°C 450°C 500°C 550°C 600°C
≤ 100 687 670 647 631 608 593 577 554 523 470 400 293
100 – 160 631 612 591 577 556 542 528 507 479 429 366 268

Tempering Values (40mm Round Bar, Quenched at 925°C in Oil)

Tempering Temperature (°C) 200 250 300 350 400 450 500 550 600 650 700
Hardness (HB) 525 520 510 485 460 438 430 409 390 360 271
Hardness (HRC) 53 52.5 52 50.5 48.5 46.5 46 44 42 39 28
Tensile Strength (N/mm²) 1950 1920 1860 1780 1660 1550 1500 1430 1360 1200 900
Yield Strength (N/mm²) 1600 1600 1580 1580 1550 1480 1360 1300 1260 1050 800
Elongation A (%) 8 8 8 8 8 8.5 9 10 11 13 16
Impact Energy Kv (J) 30 30 30 30 30 32 35 40 80 100 150

Creep Properties

40CrMoV4-6 (1.7711) is specifically designed for creep resistance, offering excellent long-term performance at elevated temperatures:

Creep Rupture Strength (σR) according to EN 10269:2013

Temperature (°C) 10,000 h (N/mm²) 100,000 h (N/mm²) 200,000 h (N/mm²)
450 513 463 446
460 483 422 400
470 451 374 347
480 413 319 286
490 371 259 229
500 321 210 187
510 269 174 155
520 223 146 130
530 187 122 103
540 160

Physical Properties

40CrMoV4-6 (1.7711) offers the following physical properties that make it suitable for high-temperature applications:

Temperature-Dependent Properties

Property Units 20°C 100°C 200°C 300°C 400°C 500°C 600°C 700°C
Thermal Expansion Coefficient (10⁻⁶·K⁻¹) 10⁻⁶·K⁻¹ 11.1* 12.1* 12.9* 13.5* 13.9* 14.1* 14.5*
Modulus of Elasticity (longitudinal) GPa 211 204 196 186 177 164 127
Modulus of Elasticity (tangential) GPa 81 78 75 71 68 63 49

* Values indicate thermal expansion coefficient between 20°C and the indicated temperature

Constant Physical Properties

Property Units Value
Specific Heat Capacity J/(kg·K) 460
Thermal Conductivity W/(m·K) 33.3
Density kg/dm³ 7.85

Applications

FUSHUN METAL’s 40CrMoV4-6 (1.7711) Creep-Resisting Steel is specifically engineered for applications requiring high strength and good creep resistance at elevated temperatures:

Power Generation Applications

  • Steam turbine components
  • Gas turbine parts
  • Turbine blades and rotors operating at moderate temperatures
  • Turbine bolting
  • Generator components
  • Power plant fasteners
  • Valve stems and bodies
  • Turbine casing components

Fastener Applications

  • High-temperature bolts (similar to ASTM A193 B16)
  • Pressure vessel studs and nuts
  • High-pressure flange bolting
  • Heat exchanger fasteners
  • Steam system fasteners
  • Petrochemical plant bolting
  • Chemical processing equipment fasteners
  • Critical structural fasteners for elevated temperature service

Pressure Equipment Applications

  • Pressure vessel components
  • High-temperature pressure piping
  • Steam headers
  • Reactor vessel parts
  • Heat exchanger components
  • Steam chest components
  • Autoclave parts
  • Boiler components

Oil & Gas Applications

  • Wellhead components
  • Downhole tools
  • Geothermal system components
  • Refinery equipment parts
  • High-pressure valves
  • Compressor components
  • Pump shafts for high-temperature service
  • Drilling equipment components

Industrial Applications

  • Die-casting tools requiring high-temperature strength
  • Forging dies for high-temperature service
  • Industrial furnace components
  • Glass industry equipment
  • Extrusion press components
  • Rolling mill parts
  • Plastic molding tools for high-temperature polymers
  • Bearings for elevated temperature service

Heat Treatment Recommendations

For customers performing their own heat treatment of 40CrMoV4-6 (1.7711) steel, FUSHUN METAL recommends the following parameters based on EN 10269:2013 standard:

Normalizing

  • Heat to 880-900°C (1615-1650°F)
  • Hold for sufficient time to ensure thorough heating
  • Cool in still air
  • Purpose: To refine grain structure and improve mechanical properties

Annealing

  • Soft Annealing: 680-730°C (1255-1345°F), slow cooling in air
  • Isothermal Annealing: 880°C (1615°F), furnace cooling to 730°C (1345°F), then air cooling
  • Spheroidized Annealing: 830°C (1525°F), slow furnace cooling
  • Resulting hardness: 220-241 HB
  • Purpose: To improve machinability and prepare for subsequent hardening

Hardening

  • Austenitizing: 900-970°C (1650-1780°F)
  • Holding time: Sufficient time for complete through-heating
  • Quenching: Oil or polymer quench
  • Achievable hardness after quenching: ~54 HRC
  • Purpose: To achieve maximum hardness and strength

Tempering

  • Temper immediately after cooling to room temperature
  • Tempering temperature: 650-720°C (1200-1330°F) for optimal creep resistance
  • Holding time: Minimum 2 hours
  • Cooling: Air cooling
  • Double tempering recommended for critical applications
  • Resulting hardness: 253-298 HB (depending on tempering temperature)
  • Purpose: To achieve required combination of strength, toughness, and creep resistance

Stress Relieving

  • Temperature: 50°C (90°F) below the tempering temperature
  • Holding time: 1-2 hours
  • Cooling: Slow cooling
  • Purpose: To relieve residual stresses from machining or welding operations

Welding Considerations

  • Pre-heating: 300°C (570°F)
  • Post-weld heat treatment: 560°C (1040°F), furnace cooling
  • Use matching composition or low-hydrogen electrodes
  • Purpose: To prevent cracking and ensure weld integrity

Machining Recommendations

To achieve optimal results when machining 40CrMoV4-6 (1.7711) steel, FUSHUN METAL recommends the following parameters:

Annealed Condition (220-241 HB)

Operation Tool Material Cutting Speed Feed Rate Depth of Cut Coolant
Turning Cemented Carbide P20-P30 120-150 m/min 0.2-0.4 mm/rev 2-5 mm Yes
Turning High Speed Steel 25-35 m/min 0.1-0.3 mm/rev 1-3 mm Yes
Milling Cemented Carbide P20-P40 100-130 m/min 0.1-0.3 mm/tooth 2-6 mm Yes
Milling High Speed Steel 20-30 m/min 0.05-0.2 mm/tooth 1-4 mm Yes
Drilling High Speed Steel 20-25 m/min 0.05-0.15 mm/rev Yes
Drilling Cemented Carbide 80-100 m/min 0.1-0.2 mm/rev Yes
Threading High Speed Steel 10-15 m/min As required Yes
Grinding Aluminum Oxide Wheel 25-30 m/sec 0.005-0.05 mm Yes

Hardened and Tempered Condition (253-298 HB)

Operation Tool Material Cutting Speed Feed Rate Depth of Cut Coolant
Turning Cemented Carbide P10-P20 80-110 m/min 0.15-0.3 mm/rev 1-3 mm Yes
Turning Ceramic Inserts 150-200 m/min 0.1-0.2 mm/rev 0.5-2 mm Optional
Milling Cemented Carbide P10-P20 70-100 m/min 0.08-0.2 mm/tooth 1-4 mm Yes
Drilling Cemented Carbide 60-80 m/min 0.08-0.15 mm/rev Yes
Threading Cemented Carbide 40-60 m/min As required Yes
Grinding Aluminum Oxide Wheel 25-30 m/sec 0.005-0.02 mm Yes

Welding Recommendations

Welding of 40CrMoV4-6 (1.7711) is possible with proper precautions:

  • Preheat: 300°C (570°F) as indicated in the technical data
  • Interpass Temperature: Maintain 300-350°C (570-660°F)
  • Post-weld Heat Treatment: Essential – 560°C (1040°F) with furnace cooling
  • Filler Materials: Matching composition or low-hydrogen electrodes
  • Processes: TIG/GTAW preferred for precision, SMAW possible with proper technique
  • Hydrogen Control: Use low hydrogen processes and consumables
  • Joint Design: Use simple joint designs with adequate access
  • Limitations: Best suited for repair welding rather than production joining
  • Alternative: Consider mechanical joining methods where possible

Comparative Advantages over Other Similar Steel Grades

Understanding how 40CrMoV4-6 (1.7711) steel compares to other grades helps in selecting the optimal material for your application:

Property 40CrMoV4-6 (1.7711) 34CrMo4 (1.7220) 30CrMoV9 (1.7707) A193 B7 (42CrMo4) X19CrMoVNbN11-1 (1.4913)
Vanadium Content 0.25-0.35% None 0.10-0.20% None 0.25-0.35%
Hot Strength Excellent Good Very Good Good Superior
Creep Resistance Excellent Moderate Good Moderate Superior
Maximum Operating Temp. 540°C 450°C 500°C 450°C 600°C
Toughness Very Good Very Good Good Very Good Moderate
Oxidation Resistance Moderate Limited Moderate Limited Excellent
Machinability Very Good Excellent Good Excellent Limited
Cost Moderate Low Moderate Low High
Typical Applications Fasteners, turbine components, pressure parts up to 540°C General engineering, medium temperature applications Pressure vessels, moderate temperature parts Standard high-strength bolting High-temperature applications to 600°C

Application-Specific Recommendations

FUSHUN METAL provides tailored recommendations for specific applications of 40CrMoV4-6 (1.7711) creep-resisting steel:

High-Temperature Fastener Applications

  • Recommended heat treatment: Quenched and tempered to achieve 850-1000 MPa tensile strength range
  • Optimal tempering temperature: 650-680°C for best combination of strength and creep resistance
  • For critical fasteners, consider 100% ultrasonic inspection to detect internal flaws
  • Thread rolling after heat treatment is recommended for improved fatigue properties
  • Apply appropriate anti-seize compound for high-temperature service
  • For steam service applications, use proper torque values accounting for thermal expansion
  • Implement proper installation procedures to ensure accurate preload
  • Consider periodic inspection and retorquing during maintenance cycles

Turbine Component Applications

  • Recommended heat treatment: Quenched and tempered to 44-46 HRC
  • For rotating parts, ensure 100% ultrasonic inspection and magnetic particle testing
  • Allow for thermal expansion in component design
  • Implement stress-relieving after major machining operations
  • For components with complex geometries, consider double tempering for maximum dimensional stability
  • Ensure surface finish requirements are met for dynamic components
  • For components under cyclic loading, shot peening may be beneficial
  • Implement appropriate non-destructive testing during regular maintenance cycles

Pressure Equipment Applications

  • Recommended heat treatment: Quenched and tempered to 285-320 HB
  • Design according to appropriate pressure vessel codes (ASME, EN, etc.)
  • For welded components, ensure proper pre-heat and post-weld heat treatment
  • Consider impact test requirements for low-temperature service
  • For pressure-containing components, 100% ultrasonic or radiographic testing recommended
  • Ensure proper allowance for corrosion and erosion in aggressive environments
  • For components subjected to thermal cycling, design to minimize thermal stress
  • Implement appropriate inspection intervals based on operating conditions

Industrial Tooling Applications

  • Recommended heat treatment: Quenched and tempered to 42-45 HRC for balanced properties
  • For hot work tools, pre-heat before use to minimize thermal shock
  • Design with proper cooling channels for temperature management
  • For dies and molds, ensure adequate support and backing
  • Consider surface treatments like nitriding for improved wear resistance
  • Implement proper preventive maintenance including regular inspection
  • For complex shapes, stress relieve after rough machining
  • Consider vacuum heat treatment for critical tooling to minimize distortion

Quality Assurance and Testing

Every batch of FUSHUN METAL’s 40CrMoV4-6 (1.7711) Steel undergoes rigorous testing to ensure it meets our exacting quality standards:

  • Chemical Composition Analysis: Spectrographic testing to verify precise element content critical for performance, with strict adherence to the allowed product deviations specified in EN 10269:2013.
  • Mechanical Property Testing: Tensile testing, hardness testing, and impact testing to verify strength, ductility, and toughness properties.
  • Microstructural Examination: Metallographic analysis to verify proper structure, grain size, and inclusion content.
  • Ultrasonic Testing: 100% ultrasonic inspection available to detect internal defects and ensure soundness.
  • Magnetic Particle Inspection: Surface inspection to detect cracks and surface defects.
  • Dimensional Verification: Precision measurement to ensure tight dimensional tolerances.
  • Heat Treatment Verification: Sample testing to confirm proper response to hardening and tempering.
  • Hardenability Testing: Jominy end-quench testing to verify through-hardening capability.
  • Elevated Temperature Testing: Verification of high-temperature mechanical properties for critical applications.
  • Cleanliness Verification: Inclusion rating to ensure premium steel quality.

Certifications Provided

  • Material Test Certificates according to EN 10204 3.1
  • Chemical composition analysis
  • Mechanical property test results
  • Dimensional inspection report
  • Heat treatment certification when applicable
  • Special property verifications available upon request
  • Certificate of conformity to ordered specifications
  • Ultrasonic testing reports when specified
  • Elevated temperature property testing when specified

Why Choose FUSHUN METAL for 40CrMoV4-6 (1.7711) Steel

When you select FUSHUN METAL as your supplier for 40CrMoV4-6 (1.7711) Steel, you partner with a leading manufacturer committed to excellence:

  • Creep-Resisting Steel Expertise: Specialized experience in manufacturing premium high-temperature steels with optimal properties.
  • Advanced Production Facilities: State-of-the-art melting, forging, and processing equipment specifically optimized for alloy steels.
  • Stringent Quality Control: Comprehensive testing and inspection protocols ensure consistent performance in demanding applications.
  • Metallurgical Knowledge: In-depth understanding of heat treatment and microstructural control of creep-resisting steels.
  • Supply Chain Reliability: Robust inventory management and production planning to ensure consistent availability of critical materials.
  • Technical Support: Expert assistance in material selection, heat treatment guidance, and application support.
  • Global Capabilities: Worldwide shipping network with experience in international documentation and compliance.
  • Material Traceability: Complete documentation and batch traceability for quality assurance.
  • Continuous Improvement: Ongoing research and development in steel processing and performance.
  • Industry Compliance: Materials and processes that meet or exceed international standards for critical applications.
  • Competitive Pricing: Excellent value combined with superior quality and service.
  • Environmental Responsibility: Commitment to sustainable manufacturing practices and environmental management.

Request Information

Contact FUSHUN METAL today to discuss your 40CrMoV4-6 (1.7711) Steel requirements. Our technical team is ready to assist you with:

  • Detailed product specifications
  • Technical consultations for your specific application
  • Heat treatment recommendations for optimal properties
  • Custom dimension and processing requirements
  • Pricing inquiries and delivery schedules
  • Sample requests for evaluation

FUSHUN METAL – Your trusted partner for premium creep-resisting steel solutions that deliver consistent quality, exceptional high-temperature performance, and excellent long-term creep resistance for the most demanding industrial applications.

 

About Us

Founded in 1998, FuShun covers an area of 3000 square meters, annual sales volume of 20000 tons. We are engaged in the manufacture and export of Tool Steel, Nickel Alloy, Stainless Steel and other special steel products…,View more content About Me.

Contact Lists

General Manager: Ms. Florence

info@fushunspecialsteel.com

Get A Free Quote!

Find your steel grade and get a quote today.

NOW Send Your Inquiry To : info@fushunspecialsteel.com

x