1. Specifications & Capability
42CrMo4 (1.7225) and AISI 4140 are the workhorse quenched and tempered (QT) alloy steels for industrial steam turbine main shafts. FUSHUN METAL open-die forges these shafts as single-piece bodies from vacuum-degassed ingots of 4.5-80 t bottom-poured or 36-114 t vacuum-cast weight on a 20/80 MN fast forging press, delivering 500-1000 mm diameter sections up to 12 m long and 100 t single weight.
The forging ratio is at least 4:1, which closes the cast structure, refines the grain and orients the metal flow along the shaft axis. Mechanical properties are verified on body samples or separately forged prolonged test pieces, so results represent the actual delivered section rather than a coupon.
| Section (mm) | Rm (MPa) | Rp0.2 (MPa) | A (%) | KV (J) |
|---|---|---|---|---|
| Up to 100 | 900-1100 | 650 min | 12 | 35 min |
| 100-250 | 750-950 | 520 min | 13 | 30 min |
| 250-500 | 700-850 | 460 min | 15 | 27 min |
| 500-1000 | 650-800 | 410 min | 15 | Verified per class |
Values follow EN 10250-3 for the 42CrMo4 QT condition; for sections above 500 mm and for ASTM A668 classes, properties are agreed and verified on separately forged prolonged test pieces. Body sampling is available on request.
2. Components & Service Conditions
These forgings serve as integral main shafts for industrial steam turbines and small turbine units, where the shaft transmits the full steam torque from the blading to the driven machine. FUSHUN METAL forges the coupling and thrust flanges as part of the shaft body, eliminating weld seams and preserving a continuous grain flow along the load path.
Service conditions combine sustained temperatures up to roughly 500 C, steady bending stress and torsional vibration. Under these loads the dominant failure mechanisms are high-cycle fatigue and long-term creep, both of which are governed by internal soundness and grain size. A forged shaft therefore offers three to five times the fatigue life of an equivalent casting, since forging closes porosity, refines the as-cast structure and eliminates shrinkage and gas defects that initiate cracks. The QT treatment provides the uniform through-section strength and low residual stress the turbine requires.
3. Grade Equivalents – 42CrMo4 / AISI 4140
| Designation | Standard | Notes |
|---|---|---|
| 42CrMo4 / 1.7225 | EN 10250-3 | European QT steel, preferred |
| AISI 4140 | SAE J404 | US equivalent |
| C45E / 1.1191 | EN 10083-2 | Plain carbon option |
| SCM440 | JIS G4105 | Japanese equivalent |
| 42ChMA | GOST 4543 | Russian equivalent |
| 40Cr | GB/T 3077 | Reference only, not used in certification |

| Grade | C | Si | Mn | Cr | Mo |
|---|---|---|---|---|---|
| 42CrMo4 (1.7225) | 0.38-0.45 | 0.40 max | 0.60-0.90 | 0.90-1.20 | 0.15-0.30 |
| AISI 4140 | 0.38-0.43 | 0.15-0.35 | 0.75-1.00 | 0.80-1.10 | 0.15-0.25 |
The chromium and molybdenum additions give 42CrMo4 its deep hardenability and temper resistance; C45E is offered where lower strength and simpler heat treatment are acceptable. FUSHUN METAL helps you select the grade against the shaft’s strength class and section size.
4. Manufacturing Process
Steelmaking. FUSHUN METAL melts in an electric arc furnace followed by ladle refining and vacuum degassing, which lowers hydrogen, oxygen and sulfur and removes non-metallic inclusions that would otherwise shorten fatigue life. Residual elements are controlled to reduce temper embrittlement in large sections.
Forging. The ingot is upset and drawn on a 20/80 MN fast forging press with a reduction ratio of at least 4:1. This closes the central porosity, breaks up the coarse cast structure and orients the grain flow along the shaft axis for maximum bending and torsional fatigue resistance.
Heat treatment. The shaft is quenched and tempered to the ordered strength and toughness, with careful control of the heating and cooling rates to achieve uniform hardness and low residual stress through the section.
Testing. Every shaft is subjected to full-section UT to EN 10228-3 and MT on machined surfaces, plus hardness and metallographic checks, with body sampling where specified. Each heat is fully traceable from ingot to final machining.
5. Standards & Certification
Turbine main shafts are supplied to EN 10250-3 (technical delivery conditions for quenched and tempered steel forgings) and ASTM A668 (general requirements for carbon and alloy steel forgings), with inspection certificates under EN 10204 3.1. A 3.2 certificate with third-party inspection is available on request.
FUSHUN METAL holds ISO 9001 and AS9120B quality system certification and can provide body sampling, additional non-destructive testing and witness points to the turbine maker’s specification. Related shaft forgings: wind turbine main shafts, hydro turbine shafts and gearbox shafts.
6. Typical Applications
Industrial steam turbines
Single-piece main shafts for small and medium industrial turbine units.
Turbine drive lines
Shafts coupling turbines to pumps, compressors and generators.
Mechanical drive trains
Rotor shafts for fans, blowers and industrial gearing packages.
Power plant spares
Replacement shafts for refurbishment and maintenance programs.
7. Inquiry Essentials
To quote your turbine main shaft, please provide the shaft drawing with diameter and length, the required strength class or hardness range, the ultrasonic testing acceptance level, the applicable standard or ASTM A668 class, and any body sampling or third-party inspection requirements.