manufacturer of nickel alloy, stainless steel, tool steel, alloy steel

K438 (IN-738LC) Master Alloy Bar for Gas Turbine Castings

Master alloy · Hot-corrosion cast superalloy · K438 / IN-738LC class

K438 Master Alloy for Gas Turbine Blades and Vanes

Built for sulphur and vanadium, not for the highest number on the data sheet. K438 carries 15.7–16.3 % chromium with tungsten, tantalum and niobium, which is why it survives the contaminated fuels and marine air that eat a higher-strength blade in a few thousand hours. We supply ingot and Ø30–250 mm bar, VIM+ESR, with sulphur held to 0.003 % where the specification asks for it.

15.7–16.3 %
Chromium
S ≤0.003 %
On request
815 °C / 421 MPa
≥70 h rupture
Ø30–250 mm
Bar diameter

At a glance

Item K438 master alloy
Designation K438 (former K38) · IN-738LC class · UNS N07738 · ЭП741
Form Cast ingot; round bar Ø30–250 mm; cut-to-length
Condition As cast, shot blasted, turned or ground
Melting route VIM+ESR as standard; VIM+ESR+VAR on request
Standards GB/T 14992 · GJB 5512.1 · AMS 2280 · ASTM B814
Certificate EN 10204 3.1 with chemistry, gas, trace elements and sulphur

The grade is chosen for one reason: it keeps its section in a dirty environment. Everything else on this page follows from that — the chromium level, the sulphur limit, the ESR route and the way acceptance is run.

Where the grade belongs, and where it does not

We are asked for K438 most often by gas turbine blade and vane suppliers, and second most often by companies who actually need K417G. The difference is the fuel. K417G is the stronger alloy at 900–950 °C and it is the right answer for clean gas. Put the same blade into a heavy-fuel machine, or onto an offshore platform where the air carries salt, and the chromium level is too low: the sulphidation front moves in from the surface and the blade fails long before its stress-rupture life is used up.

That is not a small correction. A K417 blade run on heavy fuel can lose most of its life, and the failure is not visible in the mechanical test data the buyer approved. It is visible in the deposit analysis and in the metallography of the coating interface. If the fuel specification is not on the enquiry, the first question we ask is what is being burned.

Service temperature window of K418, K438 and K417G cast superalloys
Service windows by grade. The ceiling is set by creep for K417G and by hot corrosion for K438; above 1,000 °C both give way to directionally solidified and single-crystal alloys.

Supply forms and sizes

Form Size Length Tolerance Surface Fits
Ingot 5 / 10 / 25 kg — Per mould As cast, blasted Small crucibles, single castings
Round bar Ø30–250 mm 200–1,400 mm ±1 mm dia., ±10 mm length Black, turned, ground Blade and vane castings
Cut-to-length From bar 200–700 mm ±1 mm Turned One charge, one heat

Charging practice decides the size more often than the casting does: a crucible is filled to 60–80 % of its capacity, so a 50 kg furnace takes a 25–30 kg bar. For thick-section vanes we recommend the larger bar and a cut-to-length piece rather than a stack of small ingots, because every additional piece is another surface carrying oxide into the melt.

Chemical composition

Element, % K438 (GB/T 14992) IN-738LC (typical)
C 0.10–0.20 0.09–0.13
Cr 15.7–16.3 15.7–16.3
Co 8.0–9.0 8.0–9.0
W 2.4–2.8 2.4–2.8
Mo 1.5–2.0 1.5–2.0
Al 3.2–3.7 3.2–3.7
Ti 3.0–3.5 3.2–3.7
Nb 0.6–1.1 0.6–1.1
Ta 1.5–2.0 1.5–2.0
B 0.005–0.015 0.005–0.015
Zr 0.05–0.15 0.03–0.08
Fe / Si / Mn ≤0.5 / ≤0.3 / ≤0.2 ≤0.5 / ≤0.3 / ≤0.2
P / S ≤0.015 / ≤0.015 ≤0.015 / ≤0.015

Two differences matter when a customer crosses from the Chinese designation to the American one. Carbon: the GB window runs to 0.20 % while the low-carbon 738 grade sits at 0.09–0.13 %, and carbon at the top of the window thickens the grain-boundary carbide network. Titanium: 3.0–3.5 % against 3.2–3.7 % changes the γ′ fraction slightly and the freezing range noticeably. Neither is a reason to refuse a heat; both are reasons to write the actual aim values into the order rather than the grade name.

Gas content, sulphur and inclusions

Item Aerospace / IGT grade Industrial grade
Oxygen ≤15 ppm (10 ppm on request) 30–50 ppm
Nitrogen ≤10 ppm ≤30 ppm
Sulphur ≤0.003 % (30 ppm) ≤0.015 %
O+N+S total ≤25 ppm No combined control
Pb, Bi, Sb, Sn, As, Cd ≤5 ppm each, ≤20 ppm total Per AMS 2280
Inclusion limit ≤20 µm, ≤2 per mm² Metallographic agreement

Sulphur is the number to argue about. In this alloy it does two jobs at once: it is a trace element that embrittles grain boundaries, and it is the element that reacts first with a sulphur-bearing fuel. A heat at 0.010 % is inside GB/T 14992 and still a poor starting point for a blade that will see fuel with 1 % sulphur. Getting to 30 ppm needs a low-sulphur charge and ESR; it is not a ladle addition.

Test-bar acceptance

Test Condition Requirement Reported
Tensile 800 °C σb ≥784 MPa δ5 ≥3 %
Stress rupture 815 °C / 421 MPa ≥70 h δ5
Stress rupture 850 °C / 363 MPa ≥40 h δ5
Hardness Room temperature Typical 32–38 HRC On request

As with every cast superalloy, the master alloy is not tested directly. Bars are poured from the heat under the customer’s casting practice, heat treated to the standard cycle (1120 °C solution and 850 °C ageing, for reference) and then tested. Room-temperature tensile values of 900–1,050 MPa circulate in supplier literature; they are typical values, not acceptance limits, and a purchase order should never be written against them.

Melting route and standards

Route Oxygen Relative cost Fits
VIM only 30–50 ppm 1.0 Industrial castings, short-life parts
VIM + ESR 20–30 ppm, very low S 1.3–1.5 Blades and vanes, thick sections
VIM + VAR 20–30 ppm 1.3–1.6 Conversion stock
VIM + ESR + VAR ≤10–15 ppm 1.6–2.0 Rotating parts, aerospace

For K438 the default is VIM+ESR, because the same step that drops oxygen also drops sulphur, and sulphur is the reason the grade exists. If the drawing says AMS 2280 the trace-element report comes with the heat; if it says ASTM B814 the casting acceptance route is the one being referenced, not the master alloy.

Packing, marking and traceability

  • End face — grade, heat number, melt date, net weight
  • MTC — chemistry, gas including sulphur, trace elements, standard applied, inspector and date
  • Packing — rust preventive, VCI wrap, crate with desiccant, ISPM 15 for export
  • Melt shop — disclosed on request before the order is placed

What to send with an enquiry

Send these five lines and we quote within one working day
  • Grade and standard — K438 to GB/T 14992, GJB 5512.1 or an IN-738LC drawing
  • Fuel or environment — sulphur, vanadium, salt; it decides whether K438 is the right answer at all
  • Form and size — ingot weight or bar diameter, length and single weight
  • Sulphur and gas limits — with the sampling position
  • Test bar and certificate — who pours, how often, 3.1 or 3.1 plus third-party

Email [email protected]  ·  WhatsApp +86 178 7358 1838  ·  or use the form below.

FUSHUN METAL · AS9120B · EN 10204 3.1 with the heat number.

Grades that sit next to K438

Same melting route, different balance of strength and corrosion resistance.

About Us

Founded in 1998, FuShun covers an area of 3000 square meters, annual sales volume of 20000 tons. We are engaged in the manufacture and export of Tool Steel, Nickel Alloy, Stainless Steel and other special steel products…,View more content About Me.

Contact Lists

General Manager: Ms. Florence

[email protected]

Get A Free Quote!

Find your steel grade and get a quote today.

NOW Send Your Inquiry To : [email protected]

x