Hardness conversion in one table. Brinell (HBW), Vickers (HV), Rockwell C (HRC) and tensile strength for steel from 100 to 650 HBW — what you need when a drawing calls for one scale and the mill certificate reports another.

Quick lookup: HRC to HBW, HV and tensile strength
The conversions asked for most often, taken from the full table further down.
| Rockwell C | Brinell (HBW) | Vickers (HV) | Tensile strength |
|---|---|---|---|
| 20 HRC | 228 | 240 | 770 N/mm² |
| 25 HRC | 253 | 266 | 853 N/mm² |
| 30 HRC | 286 | 301 | 968 N/mm² |
| 35 HRC | 328 | 344 | 1,110 N/mm² |
| 40 HRC | 373 | 392 | 1,263 N/mm² |
| 45 HRC | 423 | 445 | 1,437 N/mm² |
| 50 HRC | 488 | 513 | 1,677 N/mm² |
| 55 HRC | 567 | 596 | 1,982 N/mm² |
Full conversion table: 100 to 650 HBW
Every row is one Brinell step. The Rockwell column is blank below roughly 20 HRC because the C scale is not used that low — use the HRB scale there.
| Brinell Hardness | Vickers Hardness | Rockwell Hardness | Tensile Strength |
| 100 HB | 105 HV | – HRC | 335 N/mm2 |
| 101 HB | 106 HV | – HRC | 338 N/mm2 |
| 102 HB | 107 HV | – HRC | 341 N/mm2 |
| 103 HB | 108 HV | – HRC | 344 N/mm2 |
| 104 HB | 109 HV | – HRC | 347 N/mm2 |
| 105 HB | 110 HV | – HRC | 350 N/mm2 |
| 106 HB | 111 HV | – HRC | 355 N/mm2 |
| 107 HB | 112 HV | – HRC | 360 N/mm2 |
| 108 HB | 113 HV | – HRC | 365 N/mm2 |
| 109 HB | 114 HV | – HRC | 370 N/mm2 |
| 110 HB | 115 HV | – HRC | 373 N/mmø |
| 111 HB | 116 HV | – HRC | 376 N/mm2 |
| 112 HB | 117 HV | – HRC | 379 N/mm2 |
| 113 HB | 118 HV | – HRC | 382 N/mm2 |
| 114 HB | 119 HV | – HRC | 385 N/mm2 |
| 115 HB | 120 HV | – HRC | 388 N/mm2 |
| 116 HB | 121 HV | – HRC | 391 N/mm2 |
| 117 HB | 122 HV | – HRC | 394 N/mm2 |
| 118 HB | 123 HV | – HRC | 397 N/mm2 |
| 119 HB | 125 HV | – HRC | 400 N/mm2 |
| 120 HB | 126 HV | – HRC | 403 N/mm2 |
| 121 HB | 127 HV | – HRC | 406 N/mm2 |
| 122 HB | 128 HV | – HRC | 409 N/mm2 |
| 123 HB | 129 HV | – HRC | 412 N/mm2 |
| 124 HB | 130 HV | – HRC | 415 N/mm2 |
| 125 HB | 131 HV | – HRC | 418 N/mm2 |
| 126 HB | 132 HV | – HRC | 422 N/mm2 |
| 127 HB | 133 HV | – HRC | 426 N/mm2 |
| 128 HB | 135 HV | – HRC | 430 N/mm2 |
| 129 HB | 136 HV | – HRC | 434 N/mm2 |
| 130 HB | 137 HV | – HRC | 438 N/mm2 |
| 131 HB | 138 HV | – HRC | 442 N/mm2 |
| 132 HB | 139 HV | – HRC | 446 N/mm2 |
| 133 HB | 140 HV | – HRC | 450 N/mm2 |
| 134 HB | 141 HV | – HRC | 453 N/mm2 |
| 135 HB | 142 HV | – HRC | 456 N/mm2 |
| 136 HB | 143 HV | – HRC | 459 N/mm2 |
| 137 HB | 144 HV | – HRC | 462 N/mm2 |
| 138 HB | 145 HV | – HRC | 465 N/mm2 |
| 139 HB | 146 HV | – HRC | 468 N/mm2 |
| 140 HB | 147 HV | – HRC | 471 N/mm2 |
| 141 HB | 148 HV | – HRC | 474 N/mm2 |
| 142 HB | 149 HV | – HRC | 477 N/mm2 |
| 143 HB | 150 HV | – HRC | 480 N/mm2 |
| 144 HB | 151 HV | – HRC | 484 N/mm2 |
| 145 HB | 152 HV | – HRC | 488 N/mm2 |
| 146 HB | 153 HV | – HRC | 492 N/mm2 |
| 147 HB | 155 HV | – HRC | 495 N/mm2 |
| 148 HB | 156 HV | – HRC | 498 N/mm2 |
| 149 HB | 157 HV | – HRC | 501 N/mm2 |
| 150 HB | 158 HV | – HRC | 504 N/mm2 |
| 151 HB | 159 HV | – HRC | 507 N/mm2 |
| 152 HB | 160 HV | – HRC | 510 N/mm2 |
| 153 HB | 161 HV | – HRC | 515 N/mm2 |
| 154 HB | 162 HV | – HRC | 520 N/mm2 |
| 155 HB | 163 HV | – HRC | 525 N/mm2 |
| 156 HB | 164 HV | – HRC | 530 N/mm2 |
| 157 HB | 165 HV | – HRC | 532 N/mm2 |
| 158 HB | 166 HV | – HRC | 534 N/mm2 |
| 159 HB | 167 HV | – HRC | 537 N/mm2 |
| 160 HB | 168 HV | – HRC | 539 N/mm2 |
| 161 HB | 116 HV | – HRC | 542 N/mm2 |
| 162 HB | 170 HV | – HRC | 545 N/mm2 |
| 163 HB | 171 HV | – HRC | 549 N/mm2 |
| 164 HB | 172 HV | – HRC | 553 N/mm2 |
| 165 HB | 173 HV | – HRC | 557 N/mm2 |
| 166 HB | 174 HV | – HRC | 560 N/mm2 |
| 167 HB | 175 HV | – HRC | 563 N/mm2 |
| 168 HB | 176 HV | – HRC | 566 N/mm2 |
| 169 HB | 177 HV | – HRC | 569 N/mm2 |
| 170 HB | 179 HV | – HRC | 572 N/mm2 |
| 171 HB | 180 HV | – HRC | 575 N/mm2 |
| 172 HB | 181 HV | – HRC | 579 N/mm2 |
| 173 HB | 182 HV | – HRC | 583 N/mm2 |
| 174 HB | 183 HV | – HRC | 587 N/mm2 |
| 175 HB | 184 HV | – HRC | 591 N/mm2 |
| 176 HB | 185 HV | – HRC | 595 N/mm2 |
| 177 HB | 186 HV | – HRC | 598 N/mm2 |
| 178 HB | 187 HV | – HRC | 601 N/mm2 |
| 179 HB | 188 HV | – HRC | 604 N/mm2 |
| 180 HB | 189 HV | – HRC | 607 N/mm2 |
| 181 HB | 190 HV | – HRC | 610 N/mm2 |
| 182 HB | 191 HV | – HRC | 613 N/mm2 |
| 183 HB | 192 HV | – HRC | 617 N/mm2 |
| 184 HB | 193 HV | – HRC | 621 N/mm2 |
| 185 HB | 194 HV | – HRC | 625 N/mm2 |
| 186 HB | 195 HV | – HRC | 628 N/mm2 |
| 187 HB | 196 HV | – HRC | 631 N/mm2 |
| 188 HB | 197 HV | – HRC | 634 N/mm2 |
| 189 HB | 199 HV | – HRC | 637 N/mm2 |
| 190 HB | 200 HV | – HRC | 640 N/mm2 |
| 191 HB | 201 HV | – HRC | 644 N/mm2 |
| 192 HB | 202 HV | – HRC | 648 N/mm2 |
| 193 HB | 203 HV | – HRC | 652 N/mm2 |
| 194 HB | 204 HV | – HRC | 656 N/mm2 |
| 195 HB | 205 HV | – HRC | 660 N/mm2 |
| 196 HB | 206 HV | – HRC | 663 N/mm2 |
| 197 HB | 207 HV | – HRC | 667 N/mm2 |
| 198 HB | 208 HV | – HRC | 671 N/mm2 |
| 199 HB | 209 HV | – HRC | 675 N/mm2 |
| 200 HB | 210 HV | – HRC | 678 N/mm2 |
| 201 HB | 211 HV | – HRC | 681 N/mm2 |
| 202 HB | 212 HV | – HRC | 684 N/mm2 |
| 203 HB | 213 HV | – HRC | 687 N/mm2 |
| 204 HB | 214 HV | – HRC | 690 N/mm2 |
| 205 HB | 215 HV | – HRC | 693 N/mm2 |
| 206 HB | 216 HV | – HRC | 696 N/mm2 |
| 207 HB | 217 HV | – HRC | 699 N/mm2 |
| 208 HB | 218 HV | – HRC | 702 N/mm2 |
| 209 HB | 220 HV | – HRC | 705 N/mm2 |
| 210 HB | 221 HV | – HRC | 708 N/mm2 |
| 211 HB | 222 HV | – HRC | 711 N/mm2 |
| 212 HB | 223 HV | – HRC | 714 N/mm2 |
| 213 HB | 224 HV | – HRC | 717 N/mm2 |
| 214 HB | 225 HV | – HRC | 720 N/mm2 |
| 215 HB | 226 HV | – HRC | 724 N/mm2 |
| 216 HB | 227 HV | – HRC | 728 N/mm2 |
| 217 HB | 228 HV | – HRC | 732 N/mm2 |
| 218 HB | 229 HV | – HRC | 736 N/mm2 |
| 219 HB | 230 HV | – HRC | 740 N/mm2 |
| 220 HB | 231 HV | – HRC | 744 N/mm2 |
| 221 HB | 232 HV | – HRC | 748 N/mm2 |
| 222 HB | 233 HV | – HRC | 752 N/mm2 |
| 223 HB | 234 HV | – HRC | 755 N/mm2 |
| 224 HB | 235 HV | – HRC | 758 N/mm2 |
| 225 HB | 236 HV | – HRC | 761 N/mm2 |
| 226 HB | 237 HV | – HRC | 763 N/mm2 |
| 227 HB | 238 HV | – HRC | 767 N/mm2 |
| 228 HB | 240 HV | 20.3 HRC | 770 N/mm2 |
| 229 HB | 241 HV | 20.5 HRC | 773 N/mm2 |
| 230 HB | 242 HV | 20.7 HRC | 776 N/mm2 |
| 231 HB | 243 HV | 20.9 HRC | 779 N/mm2 |
| 232 HB | 244 HV | 21.1 HRC | 782 N/mm2 |
| 233 HB | 245 HV | 21.3 HRC | 785 N/mm2 |
| 234 HB | 246 HV | 21.5 HRC | 788 N/mm2 |
| 235 HB | 247 HV | 21.7 HRC | 791 N/mm2 |
| 236 HB | 248 HV | 21.9 HRC | 793 N/mm2 |
| 237 HB | 249 HV | 22.0 HRC | 797 N/mm2 |
| 238 HB | 250 HV | 22.2 HRC | 800 N/mm2 |
| 239 HB | 251 HV | 22.5 HRC | 805 N/mm2 |
| 240 HB | 252 HV | 22.7 HRC | 810 N/mm2 |
| 241 HB | 253 HV | 22.9 HRC | 815 N/mm2 |
| 242 HB | 254 HV | 23.1 HRC | 820 N/mm2 |
| 243 HB | 255 HV | 23.3 HRC | 821 N/mm2 |
| 244 HB | 256 HV | 23.5 HRC | 824 N/mm2 |
| 245 HB | 257 HV | 23.7 HRC | 827 N/mm2 |
| 246 HB | 258 HV | 23.9 HRC | 831 N/mm2 |
| 246 HB | 258 HV | 23.9 HRC | 831 N/mm2 |
| 247 HB | 260 HV | 24.0 HRC | 835 N/mm2 |
| 248 HB | 261 HV | 24.2 HRC | 838 N/mm2 |
| 249 HB | 262 HV | 24.3 HRC | 841 N/mm2 |
| 250 HB | 263 HV | 24.5 HRC | 844 N/mm2 |
| 251 HB | 264 HV | 24.7 HRC | 847 N/mm2 |
| 252 HB | 265 HV | 24.8 HRC | 850 N/mm2 |
| 253 HB | 266 HV | 25.0 HRC | 853 N/mm2 |
| 254 HB | 267 HV | 25.1 HRC | 856 N/mm2 |
| 255 HB | 268 HV | 25.3 HRC | 859 N/mm2 |
| 256 HB | 269 HV | 25.5 HRC | 862 N/mm2 |
| 257 HB | 270 HV | 25.6 HRC | 865 N/mm2 |
| 258 HB | 271 HV | 25.8 HRC | 869 N/mm2 |
| 259 HB | 272 HV | 26.0 HRC | 873 N/mm2 |
| 260 HB | 273 HV | 26.2 HRC | 877 N/mm2 |
| 261 HB | 274 HV | 26.4 HRC | 880 N/mm2 |
| 262 HB | 275 HV | 26.6 HRC | 884 N/mm2 |
| 263 HB | 276 HV | 26.7 HRC | 888 N/mm2 |
| 264 HB | 277 HV | 26.8 HRC | 892 N/mm2 |
| 265 HB | 278 HV | 26.9 HRC | 896 N/mm2 |
| 266 HB | 280 HV | 27.1 HRC | 900 N/mm2 |
| 267 HB | 281 HV | 27.3 HRC | 903 N/mm2 |
| 268 HB | 282 HV | 27.4 HRC | 906 N/mm2 |
| 269 HB | 283 HV | 27.5 HRC | 909 N/mm2 |
| 270 HB | 284 HV | 27.6 HRC | 912 N/mm2 |
| 271 HB | 285 HV | 27.8 HRC | 915 N/mm2 |
| 272 HB | 286 HV | 28.0 HRC | 918 N/mm2 |
| 273 HB | 287 HV | 28.1 HRC | 921 N/mm2 |
| 274 HB | 288 HV | 28.3 HRC | 924 N/mm2 |
| 275 HB | 289 HV | 28.4 HRC | 927 N/mm2 |
| 276 HB | 290 HV | 28.5 HRC | 930 N/mm2 |
| 277 HB | 291 HV | 28.7 HRC | 935 N/mm2 |
| 278 HB | 292 HV | 28.9 HRC | 940 N/mm2 |
| 279 HB | 293 HV | 29.0 HRC | 945 N/mm2 |
| 280 HB | 294 HV | 29.2 HRC | 950 N/mm2 |
| 281 HB | 295 HV | 29.3 HRC | 953 N/mm2 |
| 282 HB | 296 HV | 29.4 HRC | 956 N/mm2 |
| 283 HB | 297 HV | 29.5 HRC | 959 N/mm2 |
| 284 HB | 298 HV | 29.6 HRC | 962 N/mm2 |
| 285 HB | 300 HV | 29.8 HRC | 965 N/mm2 |
| 286 HB | 301 HV | 30.0 HRC | 968 N/mm2 |
| 287 HB | 302 HV | 30.2 HRC | 971 N/mm2 |
| 288 HB | 303 HV | 30.3 HRC | 974 N/mm2 |
| 289 HB | 304 HV | 30.4 HRC | 977 N/mm2 |
| 290 HB | 305 HV | 30.5 HRC | 980 N/mm2 |
| 291 HB | 306 HV | 30.6 HRC | 983 N/mm2 |
| 292 HB | 307 HV | 30.7 HRC | 986 N/mm2 |
| 293 HB | 308 HV | 30.8 HRC | 989 N/mm2 |
| 294 HB | 309 HV | 30.9 HRC | 992 N/mm2 |
| 295 HB | 310 HV | 31.0 HRC | 995 N/mm2 |
| 296 HB | 311 HV | 31.1 HRC | 999 N/mm2 |
| 297 HB | 312 HV | 31.2 HRC | 1004 N/mm2 |
| 298 HB | 313 HV | 31.3 HRC | 1008 N/mm2 |
| 299 HB | 314 HV | 31.4 HRC | 1012 N/mm2 |
| 300 HB | 315 HV | 31.6 HRC | 1015 N/mm2 |
| 301 HB | 316 HV | 31.8 HRC | 1019 N/mm2 |
| 302 HB | 317 HV | 31.9 HRC | 1013 N/mm2 |
| 303 HB | 318 HV | 32.0 HRC | 1027 N/mm2 |
| 304 HB | 320 HV | 32.2 HRC | 1030 N/mm2 |
| 305 HB | 321 HV | 32.3 HRC | 1033 N/mm2 |
| 306 HB | 322 HV | 32.4 HRC | 1036 N/mm2 |
| 307 HB | 323 HV | 32.5 HRC | 1039 N/mm2 |
| 308 HB | 324 HV | 32.6 HRC | 1042 N/mm2 |
| 309 HB | 325 HV | 32.7 HRC | 1045 N/mm2 |
| 310 HB | 326 HV | 32.8 HRC | 1048 N/mm2 |
| 311 HB | 327 HV | 32.9 HRC | 1051 N/mm2 |
| 312 HB | 328 HV | 33.0 HRC | 1054 N/mm2 |
| 312 HB | 328 HV | 33.0 HRC | 1054 N/mm2 |
| 313 HB | 329 HV | 33.1 HRC | 1057 N/mm2 |
| 314 HB | 330 HV | 33.3 HRC | 1060 N/mm2 |
| 315 HB | 331 HV | 33.4 HRC | 1063 N/mm2 |
| 316 HB | 332 HV | 33.6 HRC | 1067 N/mm2 |
| 317 HB | 333 HV | 33.7 HRC | 1071 N/mm2 |
| 318 HB | 334 HV | 33.8 HRC | 1075 N/mm2 |
| 319 HB | 335 HV | 33.9 HRC | 1079 N/mm2 |
| 320 HB | 336 HV | 34.0 HRC | 1083 N/mm2 |
| 321 HB | 337 HV | 34.1 HRC | 1087 N/mm2 |
| 322 HB | 338 HV | 34.2 HRC | 1091 N/mm2 |
| 323 HB | 339 HV | 34.4 HRC | 1095 N/mm2 |
| 324 HB | 340 HV | 34.5 HRC | 1098 N/mm2 |
| 325 HB | 341 HV | 34.6 HRC | 1101 N/mm2 |
| 326 HB | 342 HV | 34.7 HRC | 1104 N/mm2 |
| 327 HB | 343 HV | 34.9 HRC | 1107 N/mm2 |
| 328 HB | 344 HV | 35.0 HRC | 1110 N/mm2 |
| 329 HB | 345 HV | 35.1 HRC | 1113 N/mm2 |
| 330 HB | 346 HV | 35.2 HRC | 1116 N/mm2 |
| 331 HB | 347 HV | 35.3 HRC | 1119 N/mm2 |
| 332 HB | 348 HV | 35.4 HRC | 1122 N/mm2 |
| 333 HB | 350 HV | 35.5 HRC | 1125 N/mm2 |
| 334 HB | 351 HV | 35.6 HRC | 1128 N/mm2 |
| 335 HB | 352 HV | 35.7 HRC | 1131 N/mm2 |
| 336 HB | 353 HV | 35.9 HRC | 1135 N/mm2 |
| 337 HB | 354 HV | 36.0 HRC | 1138 N/mm2 |
| 338 HB | 355 HV | 36.1 HRC | 1141 N/mm2 |
| 339 HB | 356 HV | 36.2 HRC | 1145 N/mm2 |
| 340 HB | 357 HV | 36.3 HRC | 1149 N/mm2 |
| 341 HB | 358 HV | 36.4 HRC | 1152 N/mm2 |
| 342 HB | 359 HV | 36.6 HRC | 1155 N/mm2 |
| 343 HB | 360 HV | 36.7 HRC | 1158 N/mm2 |
| 344 HB | 361 HV | 36.9 HRC | 1162 N/mm2 |
| 345 HB | 362 HV | 37.0 HRC | 1165 N/mm2 |
| 346 HB | 363 HV | 37.1 HRC | 1169 N/mm2 |
| 347 HB | 364 HV | 37.2 HRC | 1172 N/mm2 |
| 348 HB | 365 HV | 37.3 HRC | 1176 N/mm2 |
| 349 HB | 366 HV | 37.4 HRC | 1179 N/mm2 |
| 350 HB | 367 HV | 37.5 HRC | 1183 N/mm2 |
| 351 HB | 368 HV | 37.6 HRC | 1187 N/mm2 |
| 352 HB | 370 HV | 37.7 HRC | 1190 N/mm2 |
| 353 HB | 371 HV | 37.8 HRC | 1194 N/mm2 |
| 354 HB | 372 HV | 38.0 HRC | 1197 N/mm2 |
| 355 HB | 373 HV | 38.1 HRC | 1201 N/mm2 |
| 356 HB | 374 HV | 38.2 HRC | 1205 N/mm2 |
| 357 HB | 375 HV | 38.4 HRC | 1208 N/mm2 |
| 358 HB | 376 HV | 38.5 HRC | 1211 N/mm2 |
| 359 HB | 377 HV | 38.6 HRC | 1214 N/mm2 |
| 360 HB | 378 HV | 38.7 HRC | 1217 N/mm2 |
| 361 HB | 380 HV | 38.8 HRC | 1220 N/mm2 |
| 362 HB | 381 HV | 38.9 HRC | 1224 N/mm2 |
| 363 HB | 382 HV | 39.0 HRC | 1227 N/mm2 |
| 364 HB | 383 HV | 39.1 HRC | 1231 N/mm2 |
| 365 HB | 384 HV | 39.2 HRC | 1234 N/mm2 |
| 366 HB | 385 HV | 39.3 HRC | 1237 N/mm2 |
| 367 HB | 386 HV | 39.4 HRC | 1241 N/mm2 |
| 368 HB | 387 HV | 39.5 HRC | 1244 N/mm2 |
| 369 HB | 388 HV | 39.6 HRC | 1247 N/mm2 |
| 370 HB | 389 HV | 39.7 HRC | 1251 N/mm2 |
| 370 HB | 389 HV | 39.7 HRC | 1251 N/mm2 |
| 371 HB | 390 HV | 39.8 HRC | 1255 N/mm2 |
| 372 HB | 391 HV | 39.9 HRC | 1259 N/mm2 |
| 373 HB | 392 HV | 40.0 HRC | 1263 N/mm2 |
| 374 HB | 393 HV | 40.1 HRC | 1267 N/mm2 |
| 375 HB | 394 HV | 40.2 HRC | 1271 N/mm2 |
| 376 HB | 395 HV | 40.3 HRC | 1275 N/mm2 |
| 377 HB | 396 HV | 40.4 HRC | 1278 N/mm2 |
| 378 HB | 397 HV | 40.5 HRC | 1282 N/mm2 |
| 379 HB | 398 HV | 40.6 HRC | 1286 N/mm2 |
| 380 HB | 400 HV | 40.8 HRC | 1290 N/mm2 |
| 381 HB | 401 HV | 40.9 HRC | 1293 N/mm2 |
| 382 HB | 402 HV | 41.0 HRC | 1296 N/mm2 |
| 383 HB | 403 HV | 41.1 HRC | 1299 N/mm2 |
| 384 HB | 404 HV | 41.2 HRC | 1302 N/mm2 |
| 385 HB | 405 HV | 41.3 HRC | 1305 N/mm2 |
| 386 HB | 406 HV | 41.4 HRC | 1308 N/mm2 |
| 387 HB | 407 HV | 41.5 HRC | 1311 N/mm2 |
| 388 HB | 408 HV | 41.6 HRC | 1314 N/mm2 |
| 389 HB | 409 HV | 41.7 HRC | 1317 N/mm2 |
| 390 HB | 410 HV | 41.8 HRC | 1320 N/mm2 |
| 391 HB | 411 HV | 41.9 HRC | 1324 N/mm2 |
| 392 HB | 412 HV | 42.0 HRC | 1328 N/mm2 |
| 393 HB | 413 HV | 42.1 HRC | 1332 N/mm2 |
| 394 HB | 414 HV | 42.2 HRC | 1335 N/mm2 |
| 395 HB | 415 HV | 42.3 HRC | 1338 N/mm2 |
| 396 HB | 416 HV | 42.4 HRC | 1342 N/mm2 |
| 397 HB | 417 HV | 42.5 HRC | 1345 N/mm2 |
| 398 HB | 418 HV | 42.6 HRC | 1347 N/mm2 |
| 399 HB | 420 HV | 42.7 HRC | 1350 N/mm2 |
| 400 HB | 421 HV | 42.8 HRC | 1353 N/mm2 |
| 401 HB | 422 HV | 42.9 HRC | 1357 N/mm2 |
| 402 HB | 423 HV | 43.0 HRC | 1360 N/mm2 |
| 403 HB | 424 HV | 43.1 HRC | 1364 N/mm2 |
| 404 HB | 425 HV | 43.2 HRC | 1367 N/mm2 |
| 405 HB | 426 HV | 43.3 HRC | 1371 N/mm2 |
| 406 HB | 427 HV | 43.4 HRC | 1373 N/mm2 |
| 407 HB | 428 HV | 43.5 HRC | 1377 N/mm2 |
| 408 HB | 429 HV | 43.5 HRC | 1381 N/mm2 |
| 409 HB | 430 HV | 43.6 HRC | 1385 N/mm2 |
| 410 HB | 431 HV | 43.7 HRC | 1389 N/mm2 |
| 411 HB | 432 HV | 43.8 HRC | 1393 N/mm2 |
| 412 HB | 433 HV | 43.9 HRC | 1397 N/mm2 |
| 413 HB | 434 HV | 44.0 HRC | 1400 N/mm2 |
| 414 HB | 435 HV | 44.1 HRC | 1404 N/mm2 |
| 415 HB | 436 HV | 44.2 HRC | 1407 N/mm2 |
| 416 HB | 437 HV | 44.3 HRC | 1411 N/mm2 |
| 417 HB | 438 HV | 44.4 HRC | 1415 N/mm2 |
| 418 HB | 440 HV | 44.5 HRC | 1420 N/mm2 |
| 419 HB | 441 HV | 44.6 HRC | 1424 N/mm2 |
| 420 HB | 442 HV | 44.7 HRC | 1427 N/mm2 |
| 421 HB | 443 HV | 44.8 HRC | 1431 N/mm2 |
| 422 HB | 444 HV | 44.9 HRC | 1434 N/mm2 |
| 423 HB | 445 HV | 45.0 HRC | 1437 N/mm2 |
| 424 HB | 446 HV | 45.1 HRC | 1441 N/mm2 |
| 425 HB | 447 HV | 45.1 HRC | 1445 N/mm2 |
| 426 HB | 448 HV | 45.2 HRC | 1448 N/mm2 |
| 427 HB | 449 HV | 45.2 HRC | 1452 N/mm2 |
| 428 HB | 450 HV | 45.3 HRC | 1455 N/mm2 |
| 429 HB | 451 HV | 45.3 HRC | 1458 N/mm2 |
| 430 HB | 452 HV | 45.4 HRC | 1461 N/mm2 |
| 431 HB | 453 HV | 45.5 HRC | 1464 N/mm2 |
| 432 HB | 454 HV | 45.6 HRC | 1468 N/mm2 |
| 433 HB | 455 HV | 45.7 HRC | 1471 N/mm2 |
| 434 HB | 456 HV | 45.8 HRC | 1474 N/mm2 |
| 435 HB | 457 HV | 45.9 HRC | 1478 N/mm2 |
| 436 HB | 458 HV | 46.0 HRC | 1482 N/mm2 |
| 437 HB | 460 HV | 46.1 HRC | 1485 N/mm2 |
| 438 HB | 461 HV | 46.2 HRC | 1488 N/mm2 |
| 439 HB | 462 HV | 46.3 HRC | 1491 N/mm2 |
| 440 HB | 463 HV | 46.4 HRC | 1494 N/mm2 |
| 441 HB | 464 HV | 46.5 HRC | 1498 N/mm2 |
| 442 HB | 465 HV | 46.6 HRC | 1502 N/mm2 |
| 443 HB | 466 HV | 46.6 HRC | 1506 N/mm2 |
| 444 HB | 467 HV | 46.7 HRC | 1509 N/mm2 |
| 445 HB | 468 HV | 46.7 HRC | 1512 N/mm2 |
| 446 HB | 469 HV | 46.8 HRC | 1516 N/mm2 |
| 447 HB | 470 HV | 46.9 HRC | 1520 N/mm2 |
| 448 HB | 471 HV | 47.0 HRC | 1524 N/mm2 |
| 449 HB | 472 HV | 47.1 HRC | 1528 N/mm2 |
| 450 HB | 473 HV | 47.1 HRC | 1532 N/mm2 |
| 451 HB | 474 HV | 47.2 HRC | 1534 N/mm2 |
| 452 HB | 475 HV | 47.3 HRC | 1538 N/mm2 |
| 453 HB | 476 HV | 47.4 HRC | 1542 N/mm2 |
| 454 HB | 477 HV | 47.5 HRC | 1546 N/mm2 |
| 455 HB | 478 HV | 47.6 HRC | 1550 N/mm2 |
| 456 HB | 480 HV | 47.7 HRC | 1555 N/mm2 |
| 457 HB | 481 HV | 47.7 HRC | 1559 N/mm2 |
| 458 HB | 482 HV | 47.8 HRC | 1563 N/mm2 |
| 459 HB | 483 HV | 47.9 HRC | 1567 N/mm2 |
| 460 HB | 484 HV | 47.9 HRC | 1571 N/mm2 |
| 461 HB | 485 HV | 48.0 HRC | 1575 N/mm2 |
| 462 HB | 486 HV | 48.1 HRC | 1579 N/mm2 |
| 463 HB | 487 HV | 48.2 HRC | 1583 N/mm2 |
| 464 HB | 488 HV | 48.3 HRC | 1587 N/mm2 |
| 465 HB | 489 HV | 48.3 HRC | 1591 N/mm2 |
| 466 HB | 490 HV | 48.4 HRC | 1595 N/mm2 |
| 467 HB | 491 HV | 48.4 HRC | 1599 N/mm2 |
| 468 HB | 492 HV | 48.5 HRC | 1603 N/mm2 |
| 469 HB | 493 HV | 48.5 HRC | 1607 N/mm2 |
| 470 HB | 494 HV | 48.6 HRC | 1611 N/mm2 |
| 471 HB | 495 HV | 48.7 HRC | 1614 N/mm2 |
| 472 HB | 496 HV | 48.8 HRC | 1618 N/mm2 |
| 473 HB | 497 HV | 48.9 HRC | 1622 N/mm2 |
| 474 HB | 498 HV | 49.0 HRC | 1626 N/mm2 |
| 475 HB | 500 HV | 49.1 HRC | 1630 N/mm2 |
| 476 HB | 501 HV | 49.2 HRC | 1633 N/mm2 |
| 477 HB | 502 HV | 49.2 HRC | 1637 N/mm2 |
| 478 HB | 503 HV | 49.3 HRC | 1640 N/mm2 |
| 479 HB | 504 HV | 49.4 HRC | 1643 N/mm2 |
| 480 HB | 505 HV | 49.5 HRC | 1644 N/mm2 |
| 481 HB | 506 HV | 49.5 HRC | 1647 N/mm2 |
| 482 HB | 507 HV | 49.6 HRC | 1651 N/mm2 |
| 483 HB | 508 HV | 49.7 HRC | 1655 N/mm2 |
| 484 HB | 509 HV | 49.7 HRC | 1660 N/mm2 |
| 485 HB | 510 HV | 49.8 HRC | 1665 N/mm2 |
| 486 HB | 511 HV | 49.9 HRC | 1669 N/mm2 |
| 487 HB | 512 HV | 49.9 HRC | 1673 N/mm2 |
| 488 HB | 513 HV | 50.0 HRC | 1677 N/mm2 |
| 489 HB | 514 HV | 50.1 HRC | 1681 N/mm2 |
| 490 HB | 515 HV | 50.2 HRC | 1685 N/mm2 |
| 491 HB | 516 HV | 50.3 HRC | 1689 N/mm2 |
| 492 HB | 517 HV | 50.3 HRC | 1693 N/mm2 |
| 493 HB | 518 HV | 50.4 HRC | 1697 N/mm2 |
| 494 HB | 520 HV | 50.5 HRC | 1700 N/mm2 |
| 495 HB | 521 HV | 50.5 HRC | 1704 N/mm2 |
| 496 HB | 522 HV | 50.6 HRC | 1708 N/mm2 |
| 497 HB | 523 HV | 50.6 HRC | 1712 N/mm2 |
| 498 HB | 524 HV | 50.7 HRC | 1716 N/mm2 |
| 499 HB | 525 HV | 50.7 HRC | 1720 N/mm2 |
| 500 HB | 526 HV | 50.8 HRC | 1724 N/mm2 |
| 501 HB | 527 HV | 50.8 HRC | 1728 N/mm2 |
| 502 HB | 528 HV | 50.9 HRC | 1732 N/mm2 |
| 503 HB | 529 HV | 51.0 HRC | 1736 N/mm2 |
| 504 HB | 530 HV | 51.1 HRC | 1740 N/mm2 |
| 505 HB | 531 HV | 51.1 HRC | 1744 N/mm2 |
| 506 HB | 532 HV | 51.2 HRC | 1748 N/mm2 |
| 507 HB | 533 HV | 51.2 HRC | 1752 N/mm2 |
| 508 HB | 534 HV | 51.3 HRC | 1756 N/mm2 |
| 509 HB | 535 HV | 51.4 HRC | 1760 N/mm2 |
| 510 HB | 536 HV | 51.5 HRC | 1764 N/mm2 |
| 511 HB | 537 HV | 51.5 HRC | 1768 N/mm2 |
| 512 HB | 538 HV | 51.6 HRC | 1772 N/mm2 |
| 513 HB | 540 HV | 51.7 HRC | 1775 N/mm2 |
| 514 HB | 541 HV | 51.7 HRC | 1779 N/mm2 |
| 515 HB | 542 HV | 51.8 HRC | 1782 N/mm2 |
| 516 HB | 543 HV | 51.8 HRC | 1786 N/mm2 |
| 517 HB | 544 HV | 51.9 HRC | 1789 N/mm2 |
| 518 HB | 545 HV | 51.9 HRC | 1793 N/mm2 |
| 519 HB | 546 HV | 52.0 HRC | 1797 N/mm2 |
| 520 HB | 547 HV | 52.0 HRC | 1801 N/mm2 |
| 521 HB | 548 HV | 52.1 HRC | 1804 N/mm2 |
| 522 HB | 549 HV | 52.2 HRC | 1807 N/mm2 |
| 523 HB | 550 HV | 52.3 HRC | 1810 N/mm2 |
| 524 HB | 551 HV | 52.3 HRC | 1814 N/mm2 |
| 525 HB | 552 HV | 52.4 HRC | 1818 N/mm2 |
| 526 HB | 553 HV | 52.4 HRC | 1822 N/mm2 |
| 527 HB | 554 HV | 52.5 HRC | 1826 N/mm2 |
| 528 HB | 555 HV | 52.6 HRC | 1830 N/mm2 |
| 529 HB | 556 HV | 52.7 HRC | 1834 N/mm2 |
| 530 HB | 557 HV | 52.8 HRC | 1838 N/mm2 |
| 531 HB | 558 HV | 52.9 HRC | 1842 N/mm2 |
| 532 HB | 560 HV | 53.0 HRC | 1845 N/mm2 |
| 533 HB | 561 HV | 53.0 HRC | 1848 N/mm2 |
| 534 HB | 562 HV | 53.1 HRC | 1852 N/mm2 |
| 535 HB | 563 HV | 53.1 HRC | 1855 N/mm2 |
| 536 HB | 564 HV | 53.2 HRC | 1859 N/mm2 |
| 537 HB | 565 HV | 53.2 HRC | 1863 N/mm2 |
| 538 HB | 566 HV | 53.3 HRC | 1867 N/mm2 |
| 539 HB | 567 HV | 53.3 HRC | 1870 N/mm2 |
| 540 HB | 568 HV | 53.4 HRC | 1873 N/mm2 |
| 541 HB | 569 HV | 53.5 HRC | 1876 N/mm2 |
| 542 HB | 570 HV | 53.6 HRC | 1880 N/mm2 |
| 543 HB | 571 HV | 53.6 HRC | 1884 N/mm2 |
| 544 HB | 571 HV | 53.7 HRC | 1889 N/mm2 |
| 545 HB | 573 HV | 53.7 HRC | 1893 N/mm2 |
| 546 HB | 574 HV | 53.8 HRC | 1898 N/mm2 |
| 547 HB | 575 HV | 53.8 HRC | 1902 N/mm2 |
| 548 HB | 576 HV | 53.9 HRC | 1907 N/mm2 |
| 549 HB | 577 HV | 53.9 HRC | 1912 N/mm2 |
| 550 HB | 578 HV | 54.0 HRC | 1916 N/mm2 |
| 551 HB | 580 HV | 54.1 HRC | 1920 N/mm2 |
| 552 HB | 581 HV | 54.1 HRC | 1923 N/mm2 |
| 553 HB | 582 HV | 54.2 HRC | 1927 N/mm2 |
| 554 HB | 583 HV | 54.2 HRC | 1930 N/mm2 |
| 555 HB | 584 HV | 54.3 HRC | 1934 N/mm2 |
| 556 HB | 585 HV | 54.3 HRC | 1937 N/mm2 |
| 557 HB | 586 HV | 54.4 HRC | 1941 N/mm2 |
| 558 HB | 587 HV | 54.4 HRC | 1945 N/mm2 |
| 559 HB | 588 HV | 54.5 HRC | 1948 N/mm2 |
| 560 HB | 589 HV | 54.6 HRC | 1952 N/mm2 |
| 561 HB | 590 HV | 54.7 HRC | 1955 N/mm2 |
| 562 HB | 591 HV | 54.7 HRC | 1959 N/mm2 |
| 563 HB | 592 HV | 54.8 HRC | 1964 N/mm2 |
| 564 HB | 593 HV | 54.8 HRC | 1969 N/mm2 |
| 565 HB | 594 HV | 54.9 HRC | 1973 N/mm2 |
| 566 HB | 595 HV | 54.9 HRC | 1978 N/mm2 |
| 567 HB | 596 HV | 55.0 HRC | 1982 N/mm2 |
| 568 HB | 597 HV | 55.1 HRC | 1987 N/mm2 |
| 569 HB | 598 HV | 55.1 HRC | 1991 N/mm2 |
| 570 HB | 600 HV | 55.2 HRC | 1995 N/mm2 |
| 571 HB | 601 HV | 55.2 HRC | 1999 N/mm2 |
| 572 HB | 602 HV | 55.3 HRC | 2002 N/mm2 |
| 573 HB | 603 HV | 55.3 HRC | 2006 N/mm2 |
| 574 HB | 604 HV | 55.4 HRC | 2009 N/mm2 |
| 575 HB | 605 HV | 55.4 HRC | 2013 N/mm2 |
| 576 HB | 606 HV | 55.5 HRC | 2016 N/mm2 |
| 577 HB | 607 HV | 55.5 HRC | 2020 N/mm2 |
| 578 HB | 608 HV | 55.6 HRC | 2023 N/mm2 |
| 579 HB | 609 HV | 55.6 HRC | 2027 N/mm2 |
| 580 HB | 610 HV | 55.7 HRC | 2030 N/mm2 |
| 581 HB | 611 HV | 55.7 HRC | 2034 N/mm2 |
| 582 HB | 612 HV | 55.8 HRC | 2039 N/mm2 |
| 583 HB | 613 HV | 55.8 HRC | 2043 N/mm2 |
| 584 HB | 614 HV | 55.9 HRC | 2048 N/mm2 |
| 585 HB | 615 HV | 55.9 HRC | 2052 N/mm2 |
| 586 HB | 616 HV | 56.0 HRC | 2057 N/mm2 |
| 587 HB | 617 HV | 56.1 HRC | 2061 N/mm2 |
| 588 HB | 618 HV | 56.2 HRC | 2065 N/mm2 |
| 589 HB | 620 HV | 56.3 HRC | 2070 N/mm2 |
| 590 HB | 621 HV | 56.3 HRC | 2073 N/mm2 |
| 591 HB | 622 HV | 56.4 HRC | 2077 N/mm2 |
| 592 HB | 623 HV | 56.4 HRC | 2080 N/mm2 |
| 593 HB | 624 HV | 56.5 HRC | 2084 N/mm2 |
| 594 HB | 625 HV | 56.5 HRC | 2087 N/mm2 |
| 595 HB | 626 HV | 56.6 HRC | 2091 N/mm2 |
| 596 HB | 627 HV | 56.6 HRC | 2093 N/mm2 |
| 597 HB | 628 HV | 56.7 HRC | 2097 N/mm2 |
| 598 HB | 629 HV | 56.7 HRC | 2101 N/mm2 |
| 599 HB | 630 HV | 56.8 HRC | 2105 N/mm2 |
| 600 HB | 631 HV | 56.8 HRC | 2109 N/mm2 |
| 601 HB | 632 HV | 56.9 HRC | 2114 N/mm2 |
| 602 HB | 633 HV | 56.9 HRC | 2118 N/mm2 |
| 603 HB | 634 HV | 57.0 HRC | 2123 N/mm2 |
| 604 HB | 635 HV | 57.0 HRC | 2127 N/mm2 |
| 605 HB | 636 HV | 57.1 HRC | 2132 N/mm2 |
| 606 HB | 637 HV | 57.2 HRC | 2136 N/mm2 |
| 607 HB | 638 HV | 57.2 HRC | 2141 N/mm2 |
| 608 HB | 640 HV | 57.3 HRC | 2145 N/mm2 |
| 609 HB | 641 HV | 57.3 HRC | 2148 N/mm2 |
| 610 HB | 642 HV | 57.4 HRC | 2152 N/mm2 |
| 611 HB | 643 HV | 57.4 HRC | 2155 N/mm2 |
| 612 HB | 644 HV | 57.5 HRC | 2159 N/mm2 |
| 613 HB | 645 HV | 57.5 HRC | 2162 N/mm2 |
| 614 HB | 646 HV | 57.6 HRC | 2166 N/mm2 |
| 615 HB | 647 HV | 57.6 HRC | 2169 N/mm2 |
| 616 HB | 648 HV | 57.7 HRC | 2173 N/mm2 |
| 617 HB | 649 HV | 57.7 HRC | 2177 N/mm2 |
| 618 HB | 650 HV | 57.8 HRC | 2180 N/mm2 |
| – HB | 651 HV | 57.8 HRC | – N/mm2 |
| – HB | 652 HV | 57.8 HRC | – N/mm2 |
| – HB | 653 HV | 57.9 HRC | – N/mm2 |
| – HB | 654 HV | 57.9 HRC | – N/mm2 |
| – HB | 655 HV | 58.0 HRC | – N/mm2 |
| – HB | 656 HV | 58.0 HRC | – N/mm2 |
| – HB | 657 HV | 58.1 HRC | – N/mm2 |
| – HB | 658 HV | 58.1 HRC | – N/mm2 |
| – HB | 660 HV | 58.3 HRC | – N/mm2 |
| – HB | 661 HV | 58.3 HRC | – N/mm2 |
| – HB | 662 HV | 58.4 HRC | – N/mm2 |
| – HB | 663 HV | 58.4 HRC | – N/mm2 |
| – HB | 664 HV | 58.5 HRC | – N/mm2 |
| – HB | 665 HV | 58.5 HRC | – N/mm2 |
| – HB | 666 HV | 58.6 HRC | – N/mm2 |
| – HB | 667 HV | 58.6 HRC | – N/mm2 |
| – HB | 668 HV | 58.7 HRC | – N/mm2 |
| – HB | 669 HV | 58.7 HRC | – N/mm2 |
| – HB | 670 HV | 58.8 HRC | – N/mm2 |
| – HB | 671 HV | 58.8 HRC | – N/mm2 |
| – HB | 672 HV | 58.9 HRC | – N/mm2 |
| – HB | 673 HV | 58.9 HRC | – N/mm2 |
| – HB | 674 HV | 59.0 HRC | – N/mm2 |
| – HB | 675 HV | 59.0 HRC | – N/mm2 |
| – HB | 676 HV | 59.0 HRC | – N/mm2 |
| – HB | 677 HV | 59.1 HRC | – N/mm2 |
| – HB | 678 HV | 59.1 HRC | – N/mm2 |
| – HB | 679 HV | 59.1 HRC | – N/mm2 |
| – HB | 680 HV | 59.2 HRC | – N/mm2 |
| – HB | 681 HV | 59.2 HRC | – N/mm2 |
| – HB | 682 HV | 59.3 HRC | – N/mm2 |
| – HB | 683 HV | 59.3 HRC | – N/mm2 |
| – HB | 684 HV | 59.4 HRC | – N/mm2 |
| – HB | 685 HV | 59.4 HRC | – N/mm2 |
| – HB | 686 HV | 59.5 HRC | – N/mm2 |
| – HB | 687 HV | 59.5 HRC | – N/mm2 |
| – HB | 688 HV | 59.6 HRC | – N/mm2 |
| – HB | 689 HV | 59.6 HRC | – N/mm2 |
| – HB | 690 HV | 59.7 HRC | – N/mm2 |
| – HB | 691 HV | 59.7 HRC | – N/mm2 |
| – HB | 692 HV | 59.8 HRC | – N/mm2 |
| – HB | 693 HV | 59.8 HRC | – N/mm2 |
| – HB | 694 HV | 59.9 HRC | – N/mm2 |
| – HB | 695 HV | 59.9 HRC | – N/mm2 |
| – HB | 696 HV | 59.9 HRC | – N/mm2 |
| – HB | 697 HV | 60.0 HRC | – N/mm2 |
| – HB | 698 HV | 60.0 HRC | – N/mm2 |
| – HB | 699 HV | 60.0 HRC | – N/mm2 |
| – HB | 700 HV | 60.1 HRC | – N/mm2 |
| – HB | 701 HV | 60.1 HRC | – N/mm2 |
| – HB | 702 HV | 60.2 HRC | – N/mm2 |
| – HB | 703 HV | 60.2 HRC | – N/mm2 |
| – HB | 704 HV | 60.2 HRC | – N/mm2 |
| – HB | 705 HV | 60.3 HRC | – N/mm2 |
| – HB | 706 HV | 60.3 HRC | – N/mm2 |
| – HB | 707 HV | 60.4 HRC | – N/mm2 |
| – HB | 708 HV | 60.4 HRC | – N/mm2 |
| – HB | 709 HV | 60.5 HRC | – N/mm2 |
| – HB | 710 HV | 60.5 HRC | – N/mm2 |
| – HB | 711 HV | 60.6 HRC | – N/mm2 |
| – HB | 712 HV | 60.6 HRC | – N/mm2 |
| – HB | 713 HV | 60.7 HRC | – N/mm2 |
| – HB | 714 HV | 60.7 HRC | – N/mm2 |
| – HB | 715 HV | 60.8 HRC | – N/mm2 |
| – HB | 716 HV | 60.8 HRC | – N/mm2 |
| – HB | 717 HV | 60.8 HRC | – N/mm2 |
| – HB | 718 HV | 60.9 HRC | – N/mm2 |
| – HB | 719 HV | 60.9 HRC | – N/mm2 |
| – HB | 720 HV | 61.0 HRC | – N/mm2 |
| – HB | 721 HV | 61.0 HRC | – N/mm2 |
| – HB | 722 HV | 61.1 HRC | – N/mm2 |
| – HB | 723 HV | 61.1 HRC | – N/mm2 |
| – HB | 724 HV | 61.2 HRC | – N/mm2 |
| – HB | 725 HV | 61.2 HRC | – N/mm2 |
| – HB | 726 HV | 61.3 HRC | – N/mm2 |
| – HB | 727 HV | 61.3 HRC | – N/mm2 |
| – HB | 728 HV | 61.4 HRC | – N/mm2 |
| – HB | 729 HV | 61.4 HRC | – N/mm2 |
| – HB | 730 HV | 61.5 HRC | – N/mm2 |
| – HB | 731 HV | 61.5 HRC | – N/mm2 |
| – HB | 732 HV | 61.6 HRC | – N/mm2 |
| – HB | 733 HV | 61.6 HRC | – N/mm2 |
| – HB | 734 HV | 61.6 HRC | – N/mm2 |
| – HB | 735 HV | 61.6 HRC | – N/mm2 |
| – HB | 736 HV | 61.7 HRC | – N/mm2 |
| – HB | 737 HV | 61.7 HRC | – N/mm2 |
| – HB | 738 HV | 61.7 HRC | – N/mm2 |
| – HB | 739 HV | 61.7 HRC | – N/mm2 |
| – HB | 740 HV | 61.8 HRC | – N/mm2 |
| – HB | 741 HV | 61.8 HRC | – N/mm2 |
| – HB | 742 HV | 61.8 HRC | – N/mm2 |
| – HB | 743 HV | 61.8 HRC | – N/mm2 |
| – HB | 744 HV | 61.9 HRC | – N/mm2 |
| – HB | 745 HV | 61.9 HRC | – N/mm2 |
| – HB | 746 HV | 61.9 HRC | – N/mm2 |
| – HB | 747 HV | 62.0 HRC | – N/mm2 |
| – HB | 748 HV | 62.0 HRC | – N/mm2 |
| – HB | 749 HV | 62.0 HRC | – N/mm2 |
| – HB | 750 HV | 62.1 HRC | – N/mm2 |
| – HB | 751 HV | 62.1 HRC | – N/mm2 |
| – HB | 752 HV | 62.1 HRC | – N/mm2 |
| – HB | 753 HV | 62.2 HRC | – N/mm2 |
| – HB | 754 HV | 62.2 HRC | – N/mm2 |
| – HB | 755 HV | 62.2 HRC | – N/mm2 |
| – HB | 756 HV | 62.3 HRC | – N/mm2 |
| – HB | 757 HV | 62.3 HRC | – N/mm2 |
| – HB | 758 HV | 62.4 HRC | – N/mm2 |
| – HB | 759 HV | 62.4 HRC | – N/mm2 |
| – HB | 760 HV | 62.5 HRC | – N/mm2 |
| – HB | 761 HV | 62.5 HRC | – N/mm2 |
| – HB | 762 HV | 62.5 HRC | – N/mm2 |
| – HB | 763 HV | 62.6 HRC | – N/mm2 |
| – HB | 764 HV | 62.6 HRC | – N/mm2 |
| – HB | 765 HV | 62.6 HRC | – N/mm2 |
| – HB | 766 HV | 62.7 HRC | – N/mm2 |
| – HB | 767 HV | 62.7 HRC | – N/mm2 |
| – HB | 768 HV | 62.7 HRC | – N/mm2 |
| – HB | 769 HV | 62.8 HRC | – N/mm2 |
| – HB | 770 HV | 62.8 HRC | – N/mm2 |
| – HB | 771 HV | 62.9 HRC | – N/mm2 |
| – HB | 772 HV | 62.9 HRC | – N/mm2 |
| – HB | 773 HV | 63.0 HRC | – N/mm2 |
| – HB | 774 HV | 63.0 HRC | – N/mm2 |
| – HB | 775 HV | 63.1 HRC | – N/mm2 |
| – HB | 776 HV | 63.1 HRC | – N/mm2 |
| – HB | 777 HV | 63.1 HRC | – N/mm2 |
| – HB | 778 HV | 63.2 HRC | – N/mm2 |
| – HB | 779 HV | 63.2 HRC | – N/mm2 |
| – HB | 780 HV | 63.3 HRC | – N/mm2 |
| – HB | 781 HV | 63.3 HRC | – N/mm2 |
| – HB | 782 HV | 63.3 HRC | – N/mm2 |
| – HB | 783 HV | 63.4 HRC | – N/mm2 |
| – HB | 784 HV | 63.4 HRC | – N/mm2 |
| – HB | 785 HV | 63.4 HRC | – N/mm2 |
| – HB | 786 HV | 63.5 HRC | – N/mm2 |
| – HB | 787 HV | 63.5 HRC | – N/mm2 |
| – HB | 788 HV | 63.5 HRC | – N/mm2 |
| – HB | 789 HV | 63.6 HRC | – N/mm2 |
| – HB | 790 HV | 63.6 HRC | – N/mm2 |
| – HB | 791 HV | 63.6 HRC | – N/mm2 |
| – HB | 792 HV | 63.7 HRC | – N/mm2 |
| – HB | 793 HV | 63.7 HRC | – N/mm2 |
| – HB | 794 HV | 63.7 HRC | – N/mm2 |
| – HB | 795 HV | 63.8 HRC | – N/mm2 |
| – HB | 796 HV | 63.8 HRC | – N/mm2 |
| – HB | 797 HV | 63.8 HRC | – N/mm2 |
| – HB | 798 HV | 63.9 HRC | – N/mm2 |
| – HB | 799 HV | 63.9 HRC | – N/mm2 |
| – HB | 800 HV | 64.0 HRC | – N/mm2 |
| – HB | 801 HV | 64.1 HRC | – N/mm2 |
| – HB | 802 HV | 64.1 HRC | – N/mm2 |
| – HB | 803 HV | 64.1 HRC | – N/mm2 |
| – HB | 804 HV | 64.2 HRC | – N/mm2 |
| – HB | 805 HV | 64.2 HRC | – N/mm2 |
| – HB | 806 HV | 64.2 HRC | – N/mm2 |
| – HB | 807 HV | 64.3 HRC | – N/mm2 |
| – HB | 808 HV | 64.3 HRC | – N/mm2 |
| – HB | 809 HV | 64.3 HRC | – N/mm2 |
| – HB | 810 HV | 64.4 HRC | – N/mm2 |
| – HB | 811 HV | 64.4 HRC | – N/mm2 |
| – HB | 812 HV | 64.4 HRC | – N/mm2 |
| – HB | 813 HV | 64.4 HRC | – N/mm2 |
| – HB | 814 HV | 64.5 HRC | – N/mm2 |
| – HB | 815 HV | 64.5 HRC | – N/mm2 |
| – HB | 816 HV | 64.5 HRC | – N/mm2 |
| – HB | 817 HV | 64.6 HRC | – N/mm2 |
| – HB | 818 HV | 64.6 HRC | – N/mm2 |
| – HB | 819 HV | 64.6 HRC | – N/mm2 |
| – HB | 820 HV | 64.7 HRC | – N/mm2 |
| – HB | 821 HV | 64.7 HRC | – N/mm2 |
| – HB | 822 HV | 64.7 HRC | – N/mm2 |
| – HB | 823 HV | 64.8 HRC | – N/mm2 |
| – HB | 824 HV | 64.8 HRC | – N/mm2 |
| – HB | 825 HV | 64.8 HRC | – N/mm2 |
| – HB | 826 HV | 64.8 HRC | – N/mm2 |
| – HB | 827 HV | 64.9 HRC | – N/mm2 |
| – HB | 828 HV | 64.9 HRC | – N/mm2 |
| – HB | 829 HV | 64.9 HRC | – N/mm2 |
| – HB | 830 HV | 65.0 HRC | – N/mm2 |
| – HB | 831 HV | 65.0 HRC | – N/mm2 |
| – HB | 832 HV | 65.0 HRC | – N/mm2 |
| – HB | 833 HV | 65.0 HRC | – N/mm2 |
| – HB | 834 HV | 65.1 HRC | – N/mm2 |
| – HB | 835 HV | 65.1 HRC | – N/mm2 |
| – HB | 836 HV | 65.1 HRC | – N/mm2 |
| – HB | 837 HV | 65.2 HRC | – N/mm2 |
| – HB | 838 HV | 65.2 HRC | – N/mm2 |
| – HB | 839 HV | 65.2 HRC | – N/mm2 |
| – HB | 840 HV | 65.3 HRC | – N/mm2 |
| – HB | 841 HV | 65.3 HRC | – N/mm2 |
| – HB | 842 HV | 65.3 HRC | – N/mm2 |
| – HB | 843 HV | 65.4 HRC | – N/mm2 |
| – HB | 844 HV | 65.4 HRC | – N/mm2 |
| – HB | 845 HV | 65.4 HRC | – N/mm2 |
| – HB | 846 HV | 65.5 HRC | – N/mm2 |
| – HB | 847 HV | 65.5 HRC | – N/mm2 |
| – HB | 848 HV | 65.5 HRC | – N/mm2 |
| – HB | 849 HV | 65.5 HRC | – N/mm2 |
| – HB | 850 HV | 65.6 HRC | – N/mm2 |
| – HB | 851 HV | 65.6 HRC | – N/mm2 |
| – HB | 852 HV | 65.6 HRC | – N/mm2 |
| – HB | 853 HV | 65.7 HRC | – N/mm2 |
| – HB | 854 HV | 65.7 HRC | – N/mm2 |
| – HB | 855 HV | 65.7 HRC | – N/mm2 |
| – HB | 856 HV | 65.8 HRC | – N/mm2 |
| – HB | 857 HV | 65.8 HRC | – N/mm2 |
| – HB | 858 HV | 65.8 HRC | – N/mm2 |
| – HB | 859 HV | 65.9 HRC | – N/mm2 |
| – HB | 860 HV | 65.9 HRC | – N/mm2 |
| – HB | 861 HV | 65.9 HRC | – N/mm2 |
| – HB | 862 HV | 65.9 HRC | – N/mm2 |
| – HB | 863 HV | 66.0 HRC | – N/mm2 |
| – HB | 864 HV | 66.0 HRC | – N/mm2 |
| – HB | 865 HV | 66.0 HRC | – N/mm2 |
| – HB | 866 HV | 66.0 HRC | – N/mm2 |
| – HB | 867 HV | 66.1 HRC | – N/mm2 |
| – HB | 868 HV | 66.1 HRC | – N/mm2 |
| – HB | 869 HV | 66.1 HRC | – N/mm2 |
| – HB | 870 HV | 66.1 HRC | – N/mm2 |
| – HB | 871 HV | 66.2 HRC | – N/mm2 |
| – HB | 872 HV | 66.2 HRC | – N/mm2 |
| – HB | 873 HV | 66.2 HRC | – N/mm2 |
| – HB | 874 HV | 66.2 HRC | – N/mm2 |
| – HB | 875 HV | 66.3 HRC | – N/mm2 |
| – HB | 876 HV | 66.3 HRC | – N/mm2 |
| – HB | 877 HV | 66.3 HRC | – N/mm2 |
| – HB | 878 HV | 66.3 HRC | – N/mm2 |
| – HB | 879 HV | 66.4 HRC | – N/mm2 |
| – HB | 880 HV | 66.4 HRC | – N/mm2 |
| – HB | 881 HV | 66.4 HRC | – N/mm2 |
| – HB | 882 HV | 66.4 HRC | – N/mm2 |
| – HB | 883 HV | 66.5 HRC | – N/mm2 |
| – HB | 884 HV | 66.5 HRC | – N/mm2 |
| – HB | 885 HV | 66.5 HRC | – N/mm2 |
| – HB | 886 HV | 66.5 HRC | – N/mm2 |
| – HB | 887 HV | 66.5 HRC | – N/mm2 |
| – HB | 888 HV | 66.6 HRC | – N/mm2 |
| – HB | 889 HV | 66.6 HRC | – N/mm2 |
| – HB | 890 HV | 66.6 HRC | – N/mm2 |
| – HB | 891 HV | 66.7 HRC | – N/mm2 |
| – HB | 892 HV | 66.7 HRC | – N/mm2 |
| – HB | 893 HV | 66.7 HRC | – N/mm2 |
| – HB | 894 HV | 66.7 HRC | – N/mm2 |
| – HB | 895 HV | 66.8 HRC | – N/mm2 |
| – HB | 896 HV | 66.8 HRC | – N/mm2 |
| – HB | 897 HV | 66.8 HRC | – N/mm2 |
| – HB | 898 HV | 66.9 HRC | – N/mm2 |
| – HB | 899 HV | 66.9 HRC | – N/mm2 |
| – HB | 900 HV | 67.0 HRC | – N/mm2 |
| – HB | 901 HV | 67.0 HRC | – N/mm2 |
| – HB | 902 HV | 67.0 HRC | – N/mm2 |
| – HB | 903 HV | 67.0 HRC | – N/mm2 |
| – HB | 904 HV | 67.0 HRC | – N/mm2 |
| – HB | 905 HV | 67.1 HRC | – N/mm2 |
| – HB | 906 HV | 67.1 HRC | – N/mm2 |
| – HB | 907 HV | 67.1 HRC | – N/mm2 |
| – HB | 908 HV | 67.1 HRC | – N/mm2 |
| – HB | 909 HV | 67.2 HRC | – N/mm2 |
| – HB | 910 HV | 67.2 HRC | – N/mm2 |
| – HB | 911 HV | 67.2 HRC | – N/mm2 |
| – HB | 912 HV | 67.2 HRC | – N/mm2 |
| – HB | 913 HV | 67.2 HRC | – N/mm2 |
| – HB | 914 HV | 67.3 HRC | – N/mm2 |
| – HB | 915 HV | 67.3 HRC | – N/mm2 |
| – HB | 916 HV | 67.3 HRC | – N/mm2 |
| – HB | 917 HV | 67.4 HRC | – N/mm2 |
| – HB | 918 HV | 67.4 HRC | – N/mm2 |
| – HB | 919 HV | 67.4 HRC | – N/mm2 |
| – HB | 920 HV | 67.5 HRC | – N/mm2 |
| – HB | 921 HV | 67.5 HRC | – N/mm2 |
| – HB | 921 HV | 67.5 HRC | – N/mm2 |
| – HB | 923 HV | 67.5 HRC | – N/mm2 |
| – HB | 924 HV | 67.6 HRC | – N/mm2 |
| – HB | 925 HV | 67.6 HRC | – N/mm2 |
| – HB | 926 HV | 67.6 HRC | – N/mm2 |
| – HB | 927 HV | 67.6 HRC | – N/mm2 |
| – HB | 928 HV | 67.7 HRC | – N/mm2 |
| – HB | 929 HV | 67.7 HRC | – N/mm2 |
| – HB | 930 HV | 67.7 HRC | – N/mm2 |
| – HB | 931 HV | 67.7 HRC | – N/mm2 |
| – HB | 932 HV | 67.8 HRC | – N/mm2 |
| – HB | 933 HV | 67.8 HRC | – N/mm2 |
| – HB | 934 HV | 67.8 HRC | – N/mm2 |
| – HB | 935 HV | 67.8 HRC | – N/mm2 |
| – HB | 936 HV | 67.9 HRC | – N/mm2 |
| – HB | 937 HV | 67.9 HRC | – N/mm2 |
| – HB | 938 HV | 67.9 HRC | – N/mm2 |
| – HB | 939 HV | 67.9 HRC | – N/mm2 |
| – HB | 940 HV | 68.0 HRC | – N/mm2 |
How to read this table
The four columns are three different test methods plus a derived value, not four measurements of the same specimen. Brinell presses a 10 mm tungsten carbide ball into the surface at 3,000 kgf and measures the indentation diameter; Vickers uses a diamond pyramid and works at any hardness; Rockwell C uses a 120° diamond cone at 150 kgf and reads depth rather than area. Tensile strength is not measured at all — it is estimated from hardness using an empirical ratio, which is why it carries the largest error of the four.

Two naming details matter when you read a certificate. HBW is the current designation and means a tungsten carbide ball; HB is the older one and referred to a hardened steel ball. HV is reported with its test load (HV10, HV30) and the load does change the number slightly on case-hardened or nitrided surfaces.
Where conversion stops being reliable
Hardness conversion assumes a homogeneous, isotropic steel. That assumption fails in several common cases, and quoting a converted value in those cases is a real quality risk:
Two of those exceptions are worth following up: austenitic stainless is non-magnetic because of its lattice, not because of its hardness, and quenching is what sets the as-quenched hardness that the table then converts.
- Austenitic stainless steels (304, 316, 321) work-harden instead of responding to the ratio the table was built on. Converted tensile values are not meaningful.
- Case-hardened and nitrided parts have a hardness gradient through the section. A Rockwell C reading is taken at the surface; the core may be five times softer.
- Cast irons and tool steels above 60 HRC sit outside the calibrated range, and the Brinell column stops at about 618 HBW because the ball deforms at higher hardness.
- Cold-drawn or cold-rolled stock carries residual work hardening that a conversion table cannot account for.
Where a specification is contractual, test the part. Conversion tables are for cross-checking a certificate, not for releasing material.
Related reading
- What is quenching — why cooling rate decides the hardness the table is converting.
- Tempering of steel — how temperature trades hardness for toughness after quenching.
- AISI 4130 properties — one grade where hardness and strength are tabulated side by side.
- Magnetic stainless grades — where a converted tensile value stops meaning anything.
You get chemical composition, mechanical properties and a price — with inspection certificates to EN 10204 3.1 issued against the heat number.