The same steel is sold in Britain as EN30B and 835M30, and that version is on a separate page because the specification
is genuinely different: EN30B carries a tighter carbon range and a different tempering response for the mining and
earthmoving market. If your drawing cites 1.6773 or 35NCD16, this page governs. If it cites EN30B or 835M30, use the
EN30B / 835M30 page.
35NCD16 DIN 1.6773 36NiCrMo16 QT Steel
1.6773 High-Strength Nickel-Chromium-Molybdenum Steel (36NiCrMo16)
Product Description
FUSHUN METAL’s 1.6773 (36NiCrMo16) is a premium high-nickel, chromium-molybdenum alloyed quenching and tempering steel offering an exceptional combination of ultra-high strength, excellent toughness, and superior hardenability. With a carefully engineered chemical composition featuring optimized levels of nickel (3.60-4.10%), chromium (1.60-2.00%), and molybdenum (0.25-0.45%), our 1.6773 delivers outstanding performance in the most demanding applications requiring superior mechanical properties throughout large cross-sections. This versatile steel is specifically developed for heavily loaded components in mechanical engineering, aerospace, defense, and high-performance automotive applications where exceptional strength combined with good toughness is essential. Available in round bars, flat bars, plates, and forgings, FUSHUN METAL’s 1.6773 steel provides consistent quality and reliable performance for the most critical engineering applications requiring superior mechanical properties even in large dimensions.
Material Designations and Standards
1.6773 (36NiCrMo16) conforms to the following standards:
| Standard | Designation |
|---|---|
| EN 10083-3 | 1.6773 / 36NiCrMo16 |
| Italy / UNI | 34NiCrMo16 |
| Germany / DIN | 36NiCrMo16 |
| France / AFNOR | 35NCD16 |
| UK / BS | 835M30 |
| China / GB | – |
| Russia / GOST | – |
| USA / AISI/SAE | – |
Chemical Composition
FUSHUN METAL’s 1.6773 (36NiCrMo16) Steel features the following chemical composition according to EN 10083-3:2006 standard:
| Element | Content (%) | Allowed Product Deviations |
|---|---|---|
| Carbon (C) | 0.32 – 0.39 | ±0.02 |
| Silicon (Si) | max. 0.40 | +0.03 |
| Manganese (Mn) | 0.50 – 0.80 | ±0.04 |
| Phosphorus (P) | max. 0.025 | +0.005 |
| Sulfur (S) | max. 0.025 | +0.005 |
| Chromium (Cr) | 1.60 – 2.00 | ±0.05 |
| Molybdenum (Mo) | 0.25 – 0.45 | ±0.04 |
| Nickel (Ni) | 3.60 – 4.10 | ±0.07 |
| Iron (Fe) | Balance | – |
Key Element Functions
- Nickel (3.60-4.10%): High nickel content significantly improves hardenability and toughness, especially at low temperatures. Contributes to excellent deep hardenability in large sections.
- Carbon (0.32-0.39%): Provides optimum balance between hardness and toughness after heat treatment, enabling high strength while maintaining good ductility.
- Chromium (1.60-2.00%): Enhances hardenability, improves wear resistance, and contributes to overall strength and corrosion resistance.
- Molybdenum (0.25-0.45%): Improves hardenability, prevents temper brittleness, and enhances high-temperature strength and creep resistance.
- Manganese (0.50-0.80%): Increases hardenability and contributes to overall strength and wear resistance.
- Silicon (max 0.40%): Acts as a deoxidizer during steelmaking and contributes to strength.
Heat Treatment Parameters
FUSHUN METAL’s 1.6773 (36NiCrMo16) can be supplied with various heat treatments according to customer requirements:
| Process | Temperature (°C) | Cooling Medium / Notes |
|---|---|---|
| Hot-forming | 1100-900 | – |
| Normalizing (+N) | 850 | Air |
| Quenching (+Q) | 880 | Air |
| Quenching (+Q) | 830-860 | Oil, polymer, water or salt bath (500°C) |
| Tempering (+T) | 550-650 | Air |
| Stress-relieving (+SR) | 50° under the temperature of tempering | – |
| Soft annealing (+A) | 650 | Air (HB max 269) |
| Isothermal annealing (+I) | 790 | Furnace cooling (HB max 275) |
| Full annealing | 825 | Water |
| Pre-heating welding | 250 | – |
| Stress-relieving after welding | 550 | Furnace cooling |
Critical Temperatures
| AC1 (°C) | AC3 (°C) | MS (°C) | Mf (°C) |
|---|---|---|---|
| 700 | 760 | 240 | 30 |
Available Product Forms and Dimensions
FUSHUN METAL offers 1.6773 (36NiCrMo16) Steel in a wide range of forms to meet diverse application requirements:
Round Bar Specifications
| Diameter (mm) | Standard Length (mm) | Surface Condition |
|---|---|---|
| 8 – 250 | 3000, 6000, Fixed or Random | Black, Peeled, Turned, Ground |
Flat Bar Specifications
| Thickness (mm) | Width (mm) | Standard Length (mm) | Surface Condition |
|---|---|---|---|
| 8 – 160 | 20 – 300 | 3000, 6000, Fixed or Random | Hot Rolled, Cold Drawn, Ground |
Plate Specifications
| Thickness (mm) | Width (mm) | Length (mm) | Surface Condition |
|---|---|---|---|
| 8 – 100 | Up to 2000 | Up to 6000 | Hot Rolled, Pickled, Ground |
Forged Components
| Diameter/Thickness (mm) | Weight Range | Surface Condition |
|---|---|---|
| Up to 990 | Up to 5000 kg | Black, Rough Machined, Proof Machined |
Mechanical Properties
1.6773 (36NiCrMo16) offers the following mechanical properties in quenched and tempered condition according to EN 10083-3:2006:
Hot-Rolled Mechanical Properties (Quenched and Tempered Condition)
| Size Range (mm) | Tensile Strength (N/mm²) | Yield Strength (N/mm²) min. | Elongation A (%) min. | Reduction of Area Z (%) min. | Impact Energy Kv (J) min. | Hardness (HBW) for information |
|---|---|---|---|---|---|---|
| d ≤ 16 / t ≤ 8 | 1250-1450 | 1050 | 9 | 40 | – | 370-415 |
| 16 < d ≤ 40 / 8 < t ≤ 20 | 1250-1450 | 1050 | 9 | 40 | 30 | 370-415 |
| 40 < d ≤ 100 / 20 < t ≤ 60 | 1100-1300 | 900 | 10 | 45 | 35 | 331-380 |
| 100 < d ≤ 160 / 60 < t ≤ 100 | 1000-1200 | 800 | 11 | 50 | 45 | 298-359 |
| 160 < d ≤ 250 / 100 < t ≤ 160 | 1000-1200 | 800 | 11 | 50 | 45 | 298-359 |
d = diameter, t = thickness
Forged Quenched and Tempered Properties (UNI EN 10250-3:2001)
| Size Range (mm) | Tensile Strength (N/mm²) min. | Yield Strength (N/mm²) min. | Elongation A (%) min. (L) | Elongation A (%) min. (T) | Impact Energy Kv (J) min. (L) | Impact Energy Kv (J) min. (T) | Hardness (HBW) min. |
|---|---|---|---|---|---|---|---|
| d ≤ 250 / t ≤ 160 | 1000 | 800 | 11 | 8 | 45 | 22 | 298 |
| 250 < d ≤ 500 / 160 < t ≤ 330 | 1000 | 800 | 11 | 8 | 45 | 22 | 298 |
| 500 < d ≤ 990 / 330 < t ≤ 660 | 1000 | 800 | 11 | 8 | 45 | 22 | 298 |
L = longitudinal, T = tangential, d = diameter, t = thickness
Tempering Values (10mm Round Bar, Quenched at 850°C in Oil)
| Tempering Temperature (°C) | 200 | 250 | 300 | 350 | 400 | 450 | 500 | 550 | 600 | 650 |
|---|---|---|---|---|---|---|---|---|---|---|
| Hardness (HB) | 518 | 496 | 468 | 448 | 432 | 409 | 385 | 357 | 327 | 301 |
| Hardness (HRC) | 52.5 | 51 | 49 | 47.5 | 46 | 44 | 41.5 | 38.5 | 35 | 32 |
| Tensile Strength (N/mm²) | 1900 | 1820 | 1720 | 1610 | 1520 | 1420 | 1320 | 1200 | 1090 | 1000 |
| Yield Strength (N/mm²) | 1550 | 1500 | 1430 | 1360 | 1290 | 1200 | 1100 | 990 | 900 | 870 |
| Elongation A (%) | 7.0 | 8.0 | 8.6 | 9.2 | 9.6 | 10.0 | 11.0 | 12.4 | 14.0 | 14.0 |
| Reduction of Area Z (%) | 23 | 24 | 25 | 27 | 27 | 28 | 32 | 38 | 48 | 50 |
| Impact Energy Kv (J) | 28 | 28 | 27 | 26 | 26 | 26 | 28 | 38 | 64 | 64 |
Hardenability
1.6773 (36NiCrMo16) features excellent deep hardenability, making it suitable for large section components requiring uniform mechanical properties throughout the cross-section.
Jominy Test Results (EN 10083-3:2006, HRC, Grain Size 5 min.)
| Distance from Quenched End (mm) | 1.5 | 3 | 5 | 7 | 9 | 11 | 13 | 15 | 20 | 25 | 30 | 35 | 40 | 45 | 50 | H |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Minimum HRC | 50 | 49 | 48 | 48 | 48 | 48 | 47 | 47 | 47 | 47 | 47 | 47 | 47 | 47 | 47 | – |
| Maximum HRC | 57 | 56 | 56 | 56 | 56 | 56 | 55 | 55 | 55 | 55 | 55 | 55 | 55 | 55 | 55 | – |
Large Section Performance (Lucefin Experience)
Forged round 300 mm quenched at 870°C in water, tempered 590°C air
| Depth from Surface | Tensile Strength (N/mm²) | Yield Strength (N/mm²) | Elongation A (%) | Reduction of Area Z (%) | Impact Energy Kv +20°C (J) | Impact Energy Kv -20°C (J) | Hardness (HB) |
|---|---|---|---|---|---|---|---|
| ½ radius | 1201 | 1110 | 12.8 | 55.0 | 90-98-90 | 62-58-60 | 371 |
Chemical Composition of Tested Forging
| C% | Si% | Mn% | P% | S% | Cr% | Mo% | Ni% |
|---|---|---|---|---|---|---|---|
| 0.34 | 0.25 | 0.50 | 0.012 | 0.005 | 1.68 | 0.40 | 3.70 |
Physical Properties
1.6773 (36NiCrMo16) offers the following physical properties:
Temperature-Dependent Properties
| Property | Units | 20°C | 100°C | 200°C | 300°C | 400°C | 500°C | 600°C |
|---|---|---|---|---|---|---|---|---|
| Thermal Expansion Coefficient | 10⁻⁶·K⁻¹ | – | 11.5* | 12.3* | 12.8* | 13.3* | 13.7* | 14.0* |
* Values indicate thermal expansion coefficient between 20°C and the indicated temperature
Constant Physical Properties
| Property | Units | Value |
|---|---|---|
| Modulus of Elasticity (longitudinal) | GPa | 208 |
| Modulus of Elasticity (tangential) | GPa | 80 |
| Specific Heat Capacity | J/(kg·K) | 460 |
| Thermal Conductivity | W/(m·K) | 33 |
| Density | kg/dm³ | 7.84 |
| Specific Electric Resistance | Ohm·mm²/m | 0.30 |
| Electrical Conductivity | Siemens·m/mm² | 3.33 |
Main Applications
1.6773 (36NiCrMo16) is specifically designed for applications requiring exceptional strength combined with good toughness, particularly in large cross-sections:
- Aerospace and Defense: Landing gear components, structural parts, high-stress aerospace components
- Automotive Industry: High-performance racing components, heavy-duty axles, transmission shafts, connecting rods
- Heavy Machinery: Large shafts, gears, and rollers for mining and construction equipment
- Energy Sector: Critical components for power generation, turbine shafts, critical fasteners
- Oil and Gas: High-pressure components, drilling equipment, large diameter connectors
- Marine Applications: Heavy-duty propeller shafts, large marine components
- Tool and Die: Large die-holders, press tooling, and forming tools
- Industrial Equipment: High-stress machine components, industrial gears, large bearings
- Railway Industry: Critical components for rolling stock and infrastructure
Machining Recommendations
To achieve optimal results when machining 1.6773 (36NiCrMo16) steel, FUSHUN METAL recommends the following parameters:
Annealed Condition (≤ 275 HB)
| Operation | Tool Material | Cutting Speed | Feed Rate | Coolant |
|---|---|---|---|---|
| Turning | Cemented Carbide P20-P30 | 100-130 m/min | 0.2-0.4 mm/rev | Yes |
| Turning | High Speed Steel | 15-25 m/min | 0.1-0.3 mm/rev | Yes |
| Milling | Cemented Carbide P20-P40 | 90-120 m/min | 0.1-0.3 mm/tooth | Yes |
| Drilling | High Speed Steel | 15-20 m/min | 0.05-0.15 mm/rev | Yes |
| Grinding | Aluminum Oxide Wheel | 25-30 m/sec | – | Yes |
Quenched and Tempered Condition (300-415 HB)
| Operation | Tool Material | Cutting Speed | Feed Rate | Coolant |
|---|---|---|---|---|
| Turning | Cemented Carbide P10-P20 | 60-80 m/min | 0.1-0.2 mm/rev | Yes |
| Milling | Cemented Carbide P10-P20 | 50-70 m/min | 0.05-0.15 mm/tooth | Yes |
| Drilling | Cemented Carbide | 40-60 m/min | 0.05-0.12 mm/rev | Yes |
| Grinding | Aluminum Oxide Wheel | 25-30 m/sec | – | Yes |
Welding Recommendations
Welding of 1.6773 (36NiCrMo16) requires special precautions due to its high alloy content:
- Preheat: 250°C as indicated in the technical data
- Post-weld Heat Treatment: Essential – 550°C with furnace cooling
- Filler Materials: Matching composition or low-hydrogen electrodes
- Processes: TIG/GTAW preferred for precision
- Hydrogen Control: Use low hydrogen processes and consumables
- Cooling Rate: Control cooling rate to avoid cracking
- Limitations: Generally not recommended for structural welding; best suited for repair welding
- Quality Control: Non-destructive testing after welding is recommended
Comparative Advantages
Understanding how 1.6773 (36NiCrMo16) compares to other grades helps in selecting the optimal material for your application:
| Property | 1.6773 (36NiCrMo16) | 1.6580 (30CrNiMo8) | 1.7225 (42CrMo4) |
|---|---|---|---|
| Nickel Content | 3.60-4.10% | 1.80-2.20% | None |
| Strength Level | Ultra High | Very High | High |
| Hardenability | Superior | Excellent | Good |
| Large Section Capability | Excellent | Very Good | Moderate |
| Low Temperature Toughness | Excellent | Very Good | Good |
| Fatigue Resistance | Excellent | Very Good | Good |
| Cost | High | Medium-High | Medium |
| Typical Applications | Aerospace, large critical components, high-stress applications | Heavy machinery, automotive components | General engineering, moderate stress applications |
Advantages of 1.6773 (36NiCrMo16)
1.6773 (36NiCrMo16) offers several key advantages that make it an excellent choice for demanding applications:
- Exceptional Strength-to-Toughness Ratio: The combination of high strength (up to 1450 MPa) with good toughness makes this steel ideal for critical components.
- Superior Deep Hardenability: The high nickel content ensures excellent hardenability even in large cross-sections, maintaining consistent mechanical properties throughout.
- Excellent Fatigue Resistance: Superior performance under cyclic loading conditions, especially for large components.
- Good Low-Temperature Toughness: Maintains good impact properties at low temperatures due to high nickel content.
- Dimensional Stability: Minimal distortion during heat treatment due to balanced alloy content.
- Consistent Properties in Large Sections: Demonstrated ability to maintain high mechanical properties even in large diameter forgings (as shown in testing data for 300mm round).
- Corrosion Resistance: Better than standard alloy steels due to chromium and nickel content.
Quality Assurance
FUSHUN METAL maintains the highest quality standards for 1.6773 (36NiCrMo16) Steel:
- Material Certificates: EN 10204/3.1 certificates provided with chemical analysis and mechanical properties
- Testing: Comprehensive testing including ultrasonic testing, grain size verification, and mechanical property testing
- Hardenability Control: Jominy end-quench testing to verify hardenability according to EN 10083-3:2006
- Microstructure Analysis: Verification of proper microstructure and grain size (min. grain size 5)
- Quality Management: ISO 9001 certified production processes
- Traceability: Full traceability from raw material to finished product
- Non-Destructive Testing: Ultrasonic examination according to industry standards
Why Choose FUSHUN METAL for 1.6773 (36NiCrMo16) Steel
When you select FUSHUN METAL as your supplier for 1.6773 (36NiCrMo16) Steel, you partner with a leading manufacturer committed to excellence:
- Material Expertise: Specialized experience in manufacturing high-nickel alloy steels for demanding applications
- Advanced Production: State-of-the-art production facilities for consistent quality in complex alloy steels
- Heat Treatment Mastery: Expert capabilities in heat treating large section components for optimal properties
- Technical Support: Expert assistance in material selection and application guidance by experienced metallurgists
- Custom Solutions: Ability to meet specific requirements for dimensions, tolerances, and mechanical properties
- Quality Assurance: Comprehensive testing and inspection to ensure superior performance in critical applications
- Reliable Supply Chain: Dependable sourcing of high-quality raw materials for consistent alloy composition
Request Information
Contact FUSHUN METAL today to discuss your 1.6773 (36NiCrMo16) Steel requirements. Our technical team is ready to assist you with:
- Detailed product specifications
- Technical consultations for your specific application
- Heat treatment recommendations for optimal properties
- Custom dimension and processing requirements
- Large section capabilities and special forgings
- Pricing inquiries and delivery schedules
In the 36NiCrMo16, 35NCD16, 30NCD16, 30NiCrMo16 grades we supply:
List of equivalents and other determinations of 36NiCrMo16 – 1.6773 steel:
6773, 36 NICRMO 16, 35NCD14, 35 NCD 14, 35NICRMO14, 35 NICRMO 14, 34HN3M, 36HNM, 30NCD16, 30 NCD 16, E30NCD16, 35NCD16, 35 NCD 16, AIR 9160/C, 32HN3M, 30NICRMO16-6, 30 NICRMO 16-6, 1.6747, LW 6747, 6747, 36CH2N4MA, 36KH2N4MA, 36H2N4MA, 36Х2Н4МА, 34CHN3M, 34KHN3M, 34ХН3М, ASNA 3133, ASNA 3134, ASNA 3149, ASNA 3181, ASNA 3197, 1.6746, FE-PL75, FDMA, 30NCD16.
We also supply :
4130 , 4130 p+x , 4140 , 4330v mod , 4340 , 4145h mod , 4317
1.8509 , 1.6523 , 1.7707 , 1.6657 , 1.6587 , 1.6582 , 1.6773
For all products, please check here: Fushun products